Gallium-holmium-doped tin oxide target material and preparation method thereof

By adding gallium oxide and holmium oxide to the tin oxide target, and through a specific preparation process, the problems of conductivity and transparency of the tin oxide target are solved, and the effects of excellent conductivity and high visible light transmittance are achieved.

CN118908720AActive Publication Date: 2024-11-08XIANDAO THIN FILM MATERIALS GUANGDONG CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411019457.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-08
Estimated Expiration
2044-07-29

AI Technical Summary

Technical Problem

As transparent conductive layer materials, the existing tin oxide targets have problems with low density and poor conductivity, and it is difficult to achieve excellent conductivity and high visible light transmittance.

Method used

采用氧化镓、氧化钬和氧化锡按特定比例混合,加入分散剂和粘结剂,经过造粒、模压、冷等静压和烧结制备,调节载流子浓度和禁带宽度以改善导电性能和透明导电薄膜的可见光透过率。

Benefits of technology

The prepared gallium holmium-doped tin oxide target has excellent conductivity and high visible light transmittance. It is suitable for transparent conductive films, with a resistivity less than 2mΩ·cm and a visible light transmittance of more than 87%.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a gallium and holmium doped tin oxide target material and a preparation method thereof, the preparation method comprises the following steps: gallium oxide, holmium oxide and tin oxide are mixed, and the obtained mixture comprises the following components in percentage by mass: 0.2%-2% of gallium oxide, 0.1%-1% of holmium oxide and 97%-99.7% of tin oxide; and adding a dispersing agent, a binder and water, and carrying out granulation, mold pressing, cold isostatic pressing and sintering to obtain the gallium and holmium doped tin oxide target material. The gallium-holmium-doped tin oxide target material has the advantages of excellent conductivity, high visible light transmittance and the like, can adjust the carrier concentration and forbidden bandwidth of a thin film when being used for the transparent conductive thin film, so that the conductivity and visible light transmittance of the thin film are effectively improved, and the gallium-holmium-doped tin oxide target material has a very good application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of target material production, and in particular relates to a gallium-holmium-doped tin oxide target material and a preparation method thereof. Background Art

[0002] In the field of heterojunction solar cells (HJT), indium oxide materials are usually used as transparent conductive layers (TCO). However, due to the high price and large fluctuation of indium oxide, its application and promotion in heterojunction solar cell devices are hindered. Compared with indium oxide materials, tin dioxide is an n-type semiconductor material with a wide band gap, high temperature resistance, corrosion resistance, excellent high-temperature conductivity, and relatively cheap price. It also has special photoelectric properties and gas-sensitive properties. Therefore, it is widely used in gas-sensitive components, semiconductor components, solar cells and other fields. However, the tin oxide target materials on the market currently have defects such as low density and poor conductivity when used as TCO materials, and their photoelectric properties are often difficult to achieve the best effect. Therefore, how to obtain a tin oxide target material with excellent conductivity, high visible light transmittance and low price is of great significance for realizing the wide application of tin oxide targets. Summary of the invention

[0003] The technical problem to be solved by the present invention is to overcome the deficiencies of the prior art and provide a gallium-holmium-doped tin oxide target material with excellent conductive properties and high visible light transmittance and a preparation method thereof.

[0004] In order to solve the above technical problems, the present invention adopts the following technical solutions.

[0005] A method for preparing a gallium-holmium-doped tin oxide target comprises the following steps: (1) Gallium oxide, holmium oxide and tin oxide are mixed to obtain a mixed powder; in terms of mass percentage, gallium oxide is 0.2% to 2%, holmium oxide is 0.1% to 1%, and tin oxide is 97% to 99.7%; (2) mixing the mixed powder obtained in step (1), a dispersant, a binder and water to obtain a slurry; (3) granulating, molding, and cold isostatic pressing the slurry obtained in step (2) to obtain a target blank; (4) Sintering the target blank obtained in step (3) to obtain a gallium-holmium-doped tin oxide target.

[0006] The above preparation method is further improved, in step (3), the molding pressure is 60MPa to 100MPa.

[0007] The above preparation method is further improved in that in step (3), the pressure of the cold isostatic pressing is 200 MPa to 400 MPa.

[0008] The above preparation method is further improved, in step (4), the sintering temperature is 1200°C to 1450°C, the sintering time is 5h to 9h, and the sintering is carried out under closed conditions.

[0009] The above preparation method is further improved, in step (1), the particle size of the gallium oxide is 50nm~150nm, and the purity of the gallium oxide is 4N; the particle size of the holmium oxide is 50nm~150nm, and the purity of the holmium oxide is 4N; the particle size of the tin oxide is 50nm~150nm, and the purity of the tin oxide is 4N.

[0010] The above preparation method is further improved, in step (2), the amount of the dispersant added is 0.2% to 5% of the total mass of the mixed powder; the amount of the binder added is 0.2% to 5% of the total mass of the mixed powder; and the solid content of the slurry is 50% to 70%.

[0011] The above preparation method is further improved in that the dispersant is ammonium polyacrylate and the binder is polyvinyl butyral.

[0012] The above preparation method is further improved in that in step (3), the granulation is spray granulation.

[0013] As a general technical concept, the present invention also provides a gallium-holmium doped tin oxide target prepared by the above preparation method.

[0014] Compared with the prior art, the advantages of the present invention are: The present invention provides a method for preparing a gallium-holmium doped tin oxide target material, which uses gallium oxide, holmium oxide and tin oxide as raw materials, wherein, by mass percentage, it contains 0.2% to 2% gallium oxide, 0.1% to 1% holmium oxide and 97% to 99.7% tin oxide; then, a dispersant and a binder are added, and after granulation, molding, cold isostatic pressing and sintering, a gallium-holmium doped tin oxide target material with excellent conductive properties and high visible light transmittance can be obtained. The preparation method of the present invention can adjust the carrier concentration and bandgap width of the film by limiting the dosage ratio of gallium oxide, holmium oxide and tin oxide, thereby effectively improving the conductive properties and visible light transmittance of the transparent conductive film prepared by the tin oxide target material, and has a good application prospect. DETAILED DESCRIPTION

[0015] The present invention is further described below in conjunction with specific preferred embodiments, but the protection scope of the present invention is not limited thereby. The materials and instruments used in the following embodiments are all commercially available.

[0016] Embodiment 1: A method for preparing a gallium-holmium doped tin oxide target material of the present invention comprises the following steps: (1) 0.2 kg of gallium oxide powder, 0.1 kg of holmium oxide powder, 9.7 kg of tin oxide powder, 0.2 kg of dispersant ammonium polyacrylate, 0.2 kg of binder polyvinyl butyral and 4.6 kg of water were uniformly mixed to obtain a slurry; wherein the gallium oxide powder had a particle size of 50 nm to 150 nm and a purity of 4N, the holmium oxide powder had a particle size of 50 nm to 150 nm and a purity of 4N, and the tin oxide powder had a particle size of 50 nm to 150 nm and a purity of 4N.

[0017] (2) The slurry obtained in step (1) is subjected to spray granulation, compression molding, and cold isostatic pressing in sequence to obtain a target material blank; wherein the pressure of the compression molding is 80 MPa, and the pressure during the cold isostatic pressing process is controlled to be 200 MPa.

[0018] (3) Sinter the target blank obtained in step (2) at 1450° C. for 5 h under normal pressure, airtight and gas-free conditions to obtain a gallium-holmium-doped tin oxide target. In this embodiment, the relative density of the gallium-holmium-doped tin oxide target is 98.5%.

[0019] The gallium-holmium doped tin oxide target prepared in this embodiment was deposited on a glass substrate by radio frequency sputtering deposition to obtain a transparent conductive film having a thickness of 800nm ​​to 900nm. According to the test, the resistivity of the transparent conductive film was 0.9mΩ·cm, and the visible light transmittance at a wavelength of 650nm was 87%.

[0020] Embodiment 2: A method for preparing a gallium-holmium doped tin oxide target material of the present invention comprises the following steps: (1) 0.02 kg of gallium oxide powder, 0.01 kg of holmium oxide powder, 9.97 kg of tin oxide powder, 0.05 kg of dispersant ammonium polyacrylate, 0.05 kg of binder polyvinyl butyral and 4.9 kg of water were uniformly mixed to obtain a slurry; wherein the gallium oxide powder had a particle size of 50 nm to 150 nm and a purity of 4N, the holmium oxide powder had a particle size of 50 nm to 150 nm and a purity of 4N, and the tin oxide powder had a particle size of 50 nm to 150 nm and a purity of 4N.

[0021] (2) The slurry obtained in step (1) is subjected to spray granulation, compression molding, and cold isostatic pressing in sequence to obtain a target blank; wherein the pressure of the compression molding is 80 MPa, and the pressure during the cold isostatic pressing process is controlled to be 400 MPa.

[0022] (3) Sinter the target blank obtained in step (2) at 1270° C. for 8 h under normal pressure, airtight and gas-free conditions to obtain a gallium-holmium-doped tin oxide target. In this embodiment, the relative density of the gallium-holmium-doped tin oxide target is 98.5%.

[0023] The gallium-holmium doped tin oxide target prepared in this embodiment is deposited on a glass substrate by radio frequency sputtering deposition to obtain a transparent conductive film having a thickness of 500nm to 600nm. According to the test, the resistivity of the transparent conductive film is 2mΩ·cm, and the visible light transmittance at a wavelength of 650nm is 94%.

[0024] Embodiment 3: A method for preparing a gallium-holmium doped tin oxide target material of the present invention comprises the following steps: (1) 0.1 kg of gallium oxide powder, 0.03 kg of holmium oxide powder, 9.87 kg of tin oxide powder, 0.1 kg of dispersant ammonium polyacrylate, 0.1 kg of binder polyvinyl butyral and 4.8 kg of water were uniformly mixed to obtain a slurry; wherein the gallium oxide powder had a particle size of 50 nm to 150 nm and a purity of 4N, the holmium oxide powder had a particle size of 50 nm to 150 nm and a purity of 4N, and the tin oxide powder had a particle size of 50 nm to 150 nm and a purity of 4N.

[0025] (2) The slurry obtained in step (1) is subjected to spray granulation, compression molding, and cold isostatic pressing in sequence to obtain a target blank; wherein the pressure of the compression molding is 80 MPa, and the pressure during the cold isostatic pressing process is controlled to be 300 MPa.

[0026] (3) Sinter the target blank obtained in step (2) at 1410° C. for 6 h under normal pressure, airtight and gas-free conditions to obtain a gallium-holmium-doped tin oxide target. In this embodiment, the relative density of the gallium-holmium-doped tin oxide target is 98.5%.

[0027] The gallium-holmium doped tin oxide target prepared in this embodiment was deposited on a glass substrate by radio frequency sputtering deposition to obtain a transparent conductive film having a thickness of 700nm to 800nm. According to the test, the resistivity of the transparent conductive film was 1.3mΩ·cm, and the visible light transmittance at a wavelength of 750nm was 89%.

[0028] Embodiment 4: A method for preparing a gallium-holmium doped tin oxide target material of the present invention comprises the following steps: (1) 0.07 kg of gallium oxide powder, 0.03 kg of holmium oxide powder, 9.9 kg of tin oxide powder, 0.12 kg of dispersant ammonium polyacrylate, 0.12 kg of binder polyvinyl butyral and 4.76 kg of water were mixed uniformly to obtain a slurry; wherein the gallium oxide powder had a particle size of 50 nm to 150 nm and a purity of 4N, the holmium oxide powder had a particle size of 50 nm to 150 nm and a purity of 4N, and the tin oxide powder had a particle size of 50 nm to 150 nm and a purity of 4N.

[0029] (2) The slurry obtained in step (1) is subjected to spray granulation, compression molding, and cold isostatic pressing in sequence to obtain a target blank; wherein the pressure of the compression molding is 80 MPa, and the pressure during the cold isostatic pressing process is controlled to be 350 MPa.

[0030] (3) Sinter the target blank obtained in step (2) at 1350° C. for 7 h under normal pressure, airtight and gas-free conditions to obtain a gallium-holmium-doped tin oxide target. In this embodiment, the relative density of the gallium-holmium-doped tin oxide target is 98.5%.

[0031] The gallium-holmium doped tin oxide target prepared in this embodiment was deposited on a glass substrate by radio frequency sputtering deposition to obtain a transparent conductive film having a thickness of 800nm ​​to 900nm. According to the test, the resistivity of the transparent conductive film was 1.5mΩ·cm, and the visible light transmittance at a wavelength of 750nm was 91%.

[0032] Comparative Example 1: A method for preparing a gallium-doped tin oxide target comprises the following steps: (1) 0.2 kg of gallium oxide powder, 9.8 kg of tin oxide powder, 0.2 kg of dispersant ammonium polyacrylate, 0.2 kg of binder polyvinyl butyral and 4.6 kg of water were mixed uniformly to obtain a slurry; wherein the gallium oxide powder had a particle size of 50 nm to 150 nm and a purity of 4N, and the tin oxide powder had a particle size of 50 nm to 150 nm and a purity of 4N.

[0033] (2) The slurry obtained in step (1) is subjected to spray granulation, compression molding, and cold isostatic pressing in sequence to obtain a target material blank; wherein the pressure of the compression molding is 80 MPa, and the pressure during the cold isostatic pressing process is controlled to be 200 MPa.

[0034] (3) Under normal pressure, airtight and gas-free conditions, the target blank obtained in step (2) is sintered at 1450° C. for 5 h to obtain a gallium-doped tin oxide target. In this embodiment, the relative density of the gallium-doped tin oxide target is 93.7%.

[0035] The gallium-doped tin oxide target prepared in this comparative example was deposited on a glass substrate by radio frequency sputtering deposition to obtain a transparent conductive film having a thickness of 800nm ​​to 900nm. According to the test, the resistivity of the transparent conductive film was 63.7mΩ•cm, and the visible light transmittance at a wavelength of 650nm was 89%.

[0036] Comparative Example 2: A method for preparing a gallium-holmium doped tin oxide target comprises the following steps: (1) 0.02 kg of gallium oxide powder, 0.2 kg of holmium oxide powder, 9.78 kg of tin oxide powder, 0.05 kg of dispersant ammonium polyacrylate, 0.05 kg of binder polyvinyl butyral and 4.9 kg of water were uniformly mixed to obtain a slurry; wherein the gallium oxide powder had a particle size of 50 nm to 150 nm and a purity of 4N, the holmium oxide powder had a particle size of 50 nm to 150 nm and a purity of 4N, and the tin oxide powder had a particle size of 50 nm to 150 nm and a purity of 4N.

[0037] (2) The slurry obtained in step (1) is subjected to spray granulation, compression molding, and cold isostatic pressing in sequence to obtain a target blank; wherein the pressure of the compression molding is 80 MPa, and the pressure during the cold isostatic pressing process is controlled to be 400 MPa.

[0038] (3) Under normal pressure, airtight and gas-free conditions, the target blank obtained in step (2) is sintered at 1400° C. for 7 h to obtain a gallium-holmium-doped tin oxide target. In this embodiment, the relative density of the gallium-holmium-doped tin oxide target is 98.5%.

[0039] The tin oxide target material doped with gallium and holmium prepared in this comparative example was deposited on a glass substrate by radio frequency sputtering deposition to obtain a transparent conductive film having a thickness of 500nm to 600nm. According to the test, the resistivity of the transparent conductive film was 37.4mΩ•cm, and the visible light transmittance at a wavelength of 650nm was 82%.

[0040] Comparative Example 3: A method for preparing a gallium-holmium doped tin oxide target comprises the following steps: (1) 0.3 kg of gallium oxide powder, 0.03 kg of holmium oxide powder, 9.67 kg of tin oxide powder, 0.1 kg of dispersant ammonium polyacrylate, 0.1 kg of binder polyvinyl butyral and 4.8 kg of water were uniformly mixed to obtain a slurry; wherein the gallium oxide powder had a particle size of 50 nm to 150 nm and a purity of 4N, the holmium oxide powder had a particle size of 50 nm to 150 nm and a purity of 4N, and the tin oxide powder had a particle size of 50 nm to 150 nm and a purity of 4N.

[0041] (2) The slurry obtained in step (1) is subjected to spray granulation, compression molding, and cold isostatic pressing in sequence to obtain a target blank; wherein the pressure of the compression molding is 80 MPa, and the pressure during the cold isostatic pressing process is controlled to be 300 MPa.

[0042] (3) Sinter the target blank obtained in step (2) at 1410° C. for 6 h under normal pressure and in a gas-free atmosphere to obtain a gallium-holmium-doped tin oxide target. In this embodiment, the relative density of the gallium-holmium-doped tin oxide target is 98.8%.

[0043] The tin oxide target material doped with gallium and holmium prepared in this comparative example was deposited on a glass substrate by radio frequency sputtering deposition to obtain a transparent conductive film having a thickness of 700nm to 800nm. According to the test, the resistivity of the transparent conductive film was 140.6mΩ•cm, and the visible light transmittance at a wavelength of 750nm was 85%.

[0044] Comparative Example 4: A method for preparing a tin oxide target material doped with gallium and cerium comprises the following steps: (1) 0.07 kg of gallium oxide powder, 0.03 kg of cerium oxide powder, 9.9 kg of tin oxide powder, 0.12 kg of dispersant ammonium polyacrylate, 0.12 kg of binder polyvinyl butyral and 4.76 kg of water were mixed uniformly to obtain a slurry; wherein the gallium oxide powder had a particle size of 50 nm to 150 nm and a purity of 4N, the cerium oxide powder had a particle size of 50 nm to 150 nm and a purity of 4N, and the tin oxide powder had a particle size of 50 nm to 150 nm and a purity of 4N.

[0045] (2) The slurry obtained in step (1) is subjected to spray granulation, compression molding, and cold isostatic pressing in sequence to obtain a target blank; wherein the pressure of the compression molding is 80 MPa, and the pressure during the cold isostatic pressing process is controlled to be 350 MPa.

[0046] (3) Under normal pressure and in a gas-free atmosphere, the target blank obtained in step (2) is sintered at 1350° C. for 7 h to obtain a tin oxide target doped with gallium and cerium. In this embodiment, the relative density of the tin oxide target doped with gallium and cerium is 95.1%.

[0047] The tin oxide target material doped with gallium and holmium prepared in this comparative example was deposited on a glass substrate by radio frequency sputtering deposition to obtain a transparent conductive film having a thickness of 800nm ​​to 900nm. According to the test, the resistivity of the transparent conductive film was 7.9mΩ•cm, and the visible light transmittance at a wavelength of 750nm was 80%.

[0048] By comparing the performance data of the doped tin oxide targets prepared in Examples 1 to 4 and Comparative Examples 1 to 4, it can be seen that compared with Example 1, the relative density of the doped tin oxide target prepared without adding holmium oxide in Comparative Example 1 is reduced, the resistivity of the conductive film prepared by the target is higher, and the visible light transmittance at a wavelength of 750nm is reduced, indicating that the doping of holmium oxide can improve the density, conductivity and light transmittance of the gallium-doped tin oxide target; compared with Example 2, more holmium oxide is added in Comparative Example 2, and the resistivity of the doped tin oxide target prepared is higher, and the visible light transmittance at a wavelength of 750nm is reduced. The visible light transmittance is reduced, indicating that when the doping amount of gallium oxide is too high, it is not conducive to the conductivity and light transmittance of the doped tin oxide target; compared with Example 3, more gallium oxide is added in Comparative Example 3, and the resistivity of the prepared doped tin oxide target is higher, and the visible light transmittance at a wavelength of 750nm is reduced, indicating that when the doping amount of gallium oxide is too high, it is not conducive to the conductivity and light transmittance of the doped tin oxide target; compared with Example 4, other rare earth oxides are added in Comparative Example 4 to replace holmium oxide, and the density of the prepared tin oxide target is reduced, and it has a higher resistivity and a lower visible light transmittance. In summary, the gallium-holmium doped tin oxide target prepared in Examples 1 to 4 has a lower resistivity and a higher visible light transmittance, and the resistivity of the transparent conductive film prepared therefrom is below 2mΩ·cm, and the visible light transmittance is above 87%.

[0049] From the above results, it can be seen that the preparation method of the gallium-holmium doped tin oxide target of the present invention uses gallium oxide, holmium oxide and tin oxide as raw materials, optimizes 0.2%-2% of gallium oxide, 0.1%-1% of holmium oxide and 97%-99.7% of tin oxide, and then adds a dispersant and a binder. After granulation, molding, cold isostatic pressing and sintering, a gallium-holmium doped tin oxide target with low resistivity and high visible light transmittance can be obtained.

[0050] The above is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as above in the preferred embodiment, it is not used to limit the present invention. Any technician familiar with the art can make many possible changes and modifications to the technical solution of the present invention by using the methods and technical contents disclosed above without departing from the spirit and technical solution of the present invention, or modify it into an equivalent embodiment of equivalent changes. Therefore, any simple modification, equivalent replacement, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention, still fall within the scope of protection of the technical solution of the present invention.

Claims

1. A method for preparing a gallium-holmium doped tin oxide target, characterized in that: The following steps are involved: (1) Gallium oxide, holmium oxide and tin oxide are mixed to obtain a mixed powder; the mixed powder contains 0.2% to 2% of gallium oxide, 0.1% to 1% of holmium oxide and 97% to 99.7% of tin oxide in terms of mass percentage; (2) mixing the mixed powder obtained in step (1), a dispersant, a binder and water to obtain a slurry; (3) granulating, molding, and cold isostatic pressing the slurry obtained in step (2) to obtain a target blank; (4) Sintering the target blank obtained in step (3) to obtain a gallium-holmium-doped tin oxide target.

2. The method for preparing a gallium-holmium doped tin oxide target according to claim 1, characterized in that: In step (3), the molding pressure is 60 MPa to 100 MPa.

3. The method for preparing a gallium-holmium doped tin oxide target according to claim 2, characterized in that: In step (3), the pressure of the cold isostatic pressing is 200 MPa to 400 MPa.

4. The method for preparing a gallium-holmium doped tin oxide target according to claim 3, characterized in that: In step (4), the sintering temperature is 1200° C. to 1450° C., the sintering time is 5 h to 9 h, and the sintering is carried out under closed conditions.

5. The method for preparing a gallium-holmium doped tin oxide target according to any one of claims 1 to 4, characterized in that: In step (1), the particle size of the gallium oxide is 50nm-150nm, and the purity of the gallium oxide is 4N; the particle size of the holmium oxide is 50nm-150nm, and the purity of the holmium oxide is 4N; the particle size of the tin oxide is 50nm-150nm, and the purity of the tin oxide is 4N.

6. The method for preparing a gallium-holmium doped tin oxide target according to any one of claims 1 to 4, characterized in that: In step (2), the amount of the dispersant added is 0.2% to 5% of the total mass of the mixed powder; the amount of the binder added is 0.2% to 5% of the total mass of the mixed powder; and the solid content of the slurry is 50% to 70%.

7. The method for preparing a gallium-holmium doped tin oxide target according to claim 6, characterized in that: The dispersant is ammonium polyacrylate, and the binder is polyvinyl butyral.

8. The method for preparing a gallium-holmium doped tin oxide target according to any one of claims 1 to 4, characterized in that: In step (3), the granulation is spray granulation.

9. A gallium-holmium-doped tin oxide target, characterized in that: The method is prepared according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Gallium oxide doped tin oxide ceramic target material and preparation method thereof

    CN112723875A

  • Sputtering target, sintered body, conductive film formed by using them, organic el device, and substrate used for the organic el device

    SG114800A1

  • Transparent conductive layer manufacturing method and apparatus, sputtering target and transparent conductive layer

    TW201538764A

  • Transparent conductive film, sputtering target and substrate equipped with the transparent conductive film