Dielectric ceramic material and preparation method thereof

Through the dielectric ceramic material composed of Cam+lTimLi2nSinO (3m+3n+l), BaZrO3 and KTaO3, combined with the fine preparation process, the dielectric loss and stability of existing microwave dielectric ceramic materials in high-frequency environments are solved. It realizes microwave performance with high dielectric constant and low dielectric loss, which has commercial application value.

CN118908722AInactive Publication Date: 2024-11-08WUXI INST OF ARTS & TECH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411019213.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing microwave dielectric ceramic materials have increased dielectric loss in high-frequency environments, and the signal transmission delay and attenuation problems are prominent, and the titanate materials have problems such as poor quality factors, high sintering temperature, poor stability and consistency.

Method used

Dielectric ceramic materials composed of Cam+lTimLi2nSinO (3m+3n+l), BaZrO3 and KTaO3 are used to use the specific chemical composition and preparation process, including ball milling, prefiring, granulation, pressing, glue removal and sintering steps. Ionic water and polyvinyl alcohol solutions were used as ball milling media and binders to prepare dielectric ceramic materials with excellent dielectric properties.

Benefits of technology

The dielectric constant εr of dielectric ceramic materials is 9~11, Q×f(GHz) ≥80000GHz, and the range of τf is -10~+10.8ppm/℃, which improves the stability and repeatability of material properties. Meet green chemistry and sustainable development requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004966697070000111
    Figure BDA0004966697070000111
  • Figure BDA0004966697070000121
    Figure BDA0004966697070000121
Patent Text Reader

Abstract

The invention provides a dielectric ceramic material and a preparation method thereof, and relates to the technical field of ceramic materials, in particular to a dielectric ceramic material. The invention relates to a dielectric ceramic material, the preparation material of the dielectric ceramic material is composed of Cam + 1TimLi2nSinO (3m + 3n + 1), BaZrO3 and KTaO3, the Cam + 1TimLi2nSinO (3m + 3n + 1) is a precursor, and the chemical composition of the dielectric ceramic material prepared by the invention is xCam + 1TimLi2nSinO (3m + 3n + 1)-yBaZrO3-zKTaO3. The dielectric ceramic material prepared by the invention has the following properties: the relative dielectric constant epsilon r is 9-11, Q * f (GHz) is greater than or equal to 80000GHz, the range of Tf is-10 to + 10.8 ppm / DEG C, and the dielectric ceramic material has very high commercial application value and market prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of ceramic materials, in particular to dielectric ceramic materials, specifically to a dielectric ceramic material and a preparation method thereof. Background Art

[0002] Dielectric ceramic materials are a type of inorganic non-metallic materials with special dielectric properties, which are widely used in the electronics industry, especially in capacitors, microwave devices, sensors, etc. Dielectric ceramic materials have become an indispensable part of modern electronic technology due to their unique electrical properties, such as high dielectric constant, low dielectric loss and high insulation strength.

[0003] Microwave dielectric ceramic materials are ceramic materials used as dielectric materials in microwave frequency band circuits and perform one or more functions. They are widely used in microwave communications, radar, electronic countermeasures and other fields. With the rapid development of wireless communication technology, the operating frequency of communication equipment has expanded to the high-frequency range, and more stringent requirements have been placed on the dielectric properties of dielectric ceramic materials. In high-frequency environments, the dielectric loss of dielectric ceramic materials increases, and signal transmission delay and attenuation problems become prominent. Generally, higher dielectric constants may be accompanied by higher dielectric losses. The signal transmission time is proportional to the dielectric constant, and the quality of signal transmission requires the high Qf of the material to ensure. In addition, in wireless communication systems, frequency stability is crucial to ensure the quality and reliability of signal transmission. Temperature changes may cause frequency drift, thereby affecting signal reception and processing. τ f The value is a measure of the sensitivity of the resonant frequency to temperature changes. Over a wide temperature range, τ f The lower the value, the stronger the ability of the dielectric ceramic to maintain a constant resonant frequency, thus ensuring the performance consistency of electronic equipment at different temperatures. r and a near-zero τ f Microwave dielectric ceramics with high value have become a research hotspot in the field of electronic information materials.

[0004] Titanates are commonly used materials for microwave dielectric ceramics and have excellent dielectric properties, but they generally have problems such as poor quality factor, high sintering temperature, poor stability and consistency. Summary of the invention

[0005] In view of the deficiencies in the prior art, the present invention provides a dielectric ceramic material and a preparation method thereof.

[0006] To achieve the above objectives, the present invention is implemented through the following technical solutions: a dielectric ceramic material, comprising Ca m+ l Ti mL i 2n Si n O (3m+3n+l), BaZrO3, KTaO3, among which Ca m+l Ti mL i 2n Si n O (3m+3n+l) For the precursor.

[0007] The Ca m+l Ti mL i 2n Si n O (3m+3n+l) The precursor is composed of CaTiO3, Li2SiO3 and CaO.

[0008] The dielectric ceramic material has a chemical composition of xCa m+l T i mL i 2n Si n O (3m+3n+l) -yBaZrO 3- zKTaO3; wherein x+y+z=1, x=0.75~0.92, y=0.05~0.20, z=0.03~0.06; wherein m+n+l=1, m=0.72~0.85, n=0.12~0.25, l=0.01~0.03.

[0009] The present invention provides a method for preparing a dielectric ceramic material, comprising the following steps:

[0010] S1: Weigh the raw materials CaTiO3, Li2SiO3, and CaO with a purity of not less than 99.9%, and mix them according to the predetermined stoichiometric ratio. Add the mixed raw materials into a ball mill, use zirconium oxide balls as grinding media, and deionized water as ball milling media for the first ball milling to ensure that the raw materials are fully mixed and refined. After the ball milling is completed, the material is dried for the first time to remove excess water to obtain the first grinding material powder, and the first grinding material powder is pre-calcined. The pre-calcined material is cooled to room temperature to obtain the precursor Ca m+l Ti mL i 2n Si n O (3m+3n+l) powder;

[0011] S2: The precursor Ca prepared above m+l Ti mL i 2n Si n O (3m+3n+l)Powder and raw materials BaZrO3 and KTaO3 with a purity of more than 99.9% are added into a ball mill in proportion as the second grinding materials for mixing, zirconium oxide spheres are added as grinding spheres, deionized water is added as ball milling media, and the second ball milling is carried out. After the ball milling is completed, a second drying treatment is carried out to obtain the second grinding material powder, and the second grinding material powder is granulated, the embryo is pressed, the embryo is debinded, and sintered to obtain the dielectric ceramic material.

[0012] The diameter of the zirconia spheres in the first ball milling and the second ball milling is 3 mm.

[0013] The temperature of the first drying process and the second drying process is 120°C.

[0014] The grinding speed of the first ball milling is 120-180 rpm, and the ball milling time is 8-12 hours.

[0015] The weight ratio of the first grinding material, the zirconium oxide spheres and the deionized water is 1:2:2.

[0016] The pre-burning starts from the ambient temperature, the heating rate is 5°C / min, the pre-burning temperature range is 1100°C to 1200°C, and after reaching the target temperature, the temperature is kept for 3.5 to 4.5 hours.

[0017] The second ball milling has a grinding speed of 200 to 280 rpm and a ball milling time of 16 to 20 hours.

[0018] The weight ratio of the second grinding material, zirconium oxide spheres and deionized water is 1:2:1.5.

[0019] The specific process of the granulation treatment is to add a polyvinyl acid solution as a binder to the second grinding material powder, add 0.04-0.06 mL of a 6% polyvinyl alcohol solution per gram of powder, mix evenly, granulate, and then pass through a 120-mesh sieve to obtain the granulated powder.

[0020] The pressed embryo body is a cylindrical embryo body with a diameter of 15 mm and a height of 12 mm, which is formed by pressing the granulated powder under a pressure of 50 MPa.

[0021] The debinding of the embryo body is to place the cylindrical embryo body into a smelting furnace, set the heating rate of the smelting furnace to 5°C / min, the debinding temperature range to 400°C to 600°C, and keep the temperature for 1 to 2 hours after reaching the target temperature.

[0022] The sintering is to set the heating rate of the smelting furnace to 3°C / min after debinding, and the sintering temperature range is 1150°C to 1250°C. After reaching the target temperature, the temperature is kept for 3.5 to 5 hours.

[0023] The present invention provides a dielectric ceramic material and a preparation method thereof, which has the following beneficial effects:

[0024] 1. The present invention uses titanate as the basis and adds lithium salt to prepare Ca m+l Ti mL i 2n Si n O (3m+3n+l) Precursor, adding BaZrO3 with high thermal conductivity and high stability, and then adding LiNbO3 with excellent dielectric properties. Through the synergistic effect between the components, the material performance is significantly improved, and a dielectric ceramic material with excellent microwave performance is prepared. Its relative dielectric constant ε r 9~11, Q×f(GHz)≥80000GHz, T f The range is -10~+10.8ppm / ℃, which has very high commercial application value and market prospects.

[0025] 2. Calcination temperature is one of the key parameters in the ceramic preparation process, which has a significant impact on the final performance of the ceramic medium. The present invention adds lithium salts and dopes niobium elements to lower the sintering temperature and promote grain growth. The sintering temperature is usually between 1250°C and 1350°C. The sintering temperature in the preparation method of the present invention is usually between 1100°C and 1250°C, and the sintering is stable.

[0026] 3. The present invention ensures the consistency and repeatability of material properties through specific chemical composition and sophisticated preparation process, including precisely controlled ball milling, pre-sintering, granulation, pressing, debinding and sintering steps. The present invention uses deionized water as ball milling medium and adds polyvinyl alcohol solution as binder during granulation. These materials have little impact on the environment and meet the requirements of green chemistry and sustainable development. DETAILED DESCRIPTION

[0027] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] The present invention provides embodiments 1 to 10, and takes embodiment 1 as an example to specifically illustrate the preparation process of the present invention.

[0029] Example 1

[0030] A dielectric ceramic material, the chemical composition of which is: Ca m+l Ti mL i 2n Si n O(3m+3n+l) -yBaZrO3-zKTaO3; wherein x=0.85, y=0.12, z=0.03; m=0.75, n=0.20, l=0.05.

[0031] S1: Weigh the raw materials CaTiO3, Li2SiO3, and CaO with a purity of not less than 99.9%, and mix them according to the predetermined stoichiometric ratio. Add the mixed raw materials into a ball mill, use zirconia spheres as grinding media, and deionized water as the ball milling medium for the first ball milling. The weight ratio of the first ground material, zirconia spheres, and deionized water is 1:2:2, the grinding speed is 150rpm, and the ball milling time is 10h to ensure that the raw materials are fully mixed and refined. After the ball milling is completed, the material is dried for the first time to remove excess water to obtain the first ground material powder, and the first ground material powder is pre-calcined. The pre-calcination starts from ambient temperature, the heating rate is 5℃ / min, the pre-calcination temperature range is 1150℃, and after reaching the target temperature, it is kept warm for 4h. The pre-calcined material is cooled to room temperature to obtain the precursor Ca m+l Ti mL i 2n Si n O (3m+3n+l) powder;

[0032] S2: The precursor Ca prepared above m+l Ti mL i 2n Si n O (3m+3n+l) Powder and raw materials BaZrO3 and KTaO3 with a purity of more than 99.9% as the second grinding materials are added to the ball mill in proportion for mixing, zirconium oxide balls are added as grinding balls, deionized water is added as ball milling medium, and the second ball milling is performed. The weight ratio of the second grinding material, zirconium oxide balls, and deionized water is 1:2:1.5, the grinding speed is 240rpm, and the ball milling time is 18h. After the ball milling is completed, a second drying treatment is performed to obtain the second grinding material powder. 0.05 mL of 6% polyvinyl alcohol solution was added to each gram of powder, and the mixture was evenly mixed and granulated. The powder was then passed through a 120-mesh sieve to obtain the granulated powder. The granulated powder was pressed into a cylindrical embryo with a diameter of 15 mm and a height of 12 mm under a pressure of 50 MPa. The embryo was debinded by placing the cylindrical embryo into a smelting furnace, and the heating rate of the smelting furnace was set to 5°C / min, the debinding temperature range was 500°C, and the target temperature was reached. The temperature was kept for 1.5 hours. After debinding, the heating rate of the smelting furnace was set to 3°C / min, and the sintering temperature range was 1200°C. After reaching the target temperature, the temperature was kept for 4 hours, and the dielectric ceramic material was obtained after cooling.

[0033] Example 2

[0034] A dielectric ceramic material, the chemical composition of which is: Ca m+l Ti mL i 2n Si n O (3m+3n+l) -yBaZrO3-zKTaO3; wherein x=0.81, y=0.17, z=0.02; m=0.79, n=0.16, l=0.05.

[0035] S1: The raw materials for the first ball milling are CaTiO3, Li2SiO3, and CaO, which are mixed in a stoichiometric ratio. The ball milling medium is deionized water, the grinding speed is 120rpm, and the ball milling time is 8h. The pre-calcination temperature is 1200℃, and the temperature is kept for 3.5h.

[0036] S2: BaZrO3 and KTaO3 were added in the second ball milling, the grinding speed was 280rpm, and the ball milling time was 20h. Polyvinyl alcohol solution was added during the granulation process, and 0.06mL of 6% polyvinyl alcohol solution was added per gram of powder. The pressing pressure of the embryo was 50MPa, the cylinder diameter was 15mm, and the height was 12mm. The embryo debinding temperature was 400℃, and the temperature was kept for 1h. The sintering temperature was 1150℃, and the temperature was kept for 3.5h.

[0037] Example 3

[0038] A dielectric ceramic material, the chemical composition of which is: Ca m+l Ti mL i 2n Si n O (3m+3n+l) -yBaZrO3-zKTaO3; wherein x=0.74, y=0.24, z=0.02; m=0.88, n=0.08, l=0.04.

[0039] S1: The raw materials for the first ball milling are CaTiO3, Li2SiO3, and CaO, which are mixed in a stoichiometric ratio. The ball milling medium is deionized water, the grinding speed is 180rpm, and the ball milling time is 12h. The pre-calcination temperature is 1100℃, and the temperature is kept for 4.5h.

[0040] S2: BaZrO3 and KTaO3 were added in the second ball milling, the grinding speed was 200rpm, and the ball milling time was 16h. Polyvinyl alcohol solution was added during the granulation process, and 0.04mL of 6% polyvinyl alcohol solution was added per gram of powder. The pressing pressure of the embryo was 50MPa, the cylinder diameter was 15mm, and the height was 12mm. The embryo debinding temperature was 600℃, and the temperature was kept for 2h. The sintering temperature was 1250℃, and the temperature was kept for 5h.

[0041] Example 4

[0042] A dielectric ceramic material, the chemical composition of which is: Ca m+l TimL i 2n Si n O (3m+3n+l) -yBaZrO3-zKTaO3; wherein x=0.72, y=0.25, z=0.02; m=0.92, n=0.05, l=0.03.

[0043] S1: The raw materials for the first ball milling are CaTiO3, Li2SiO3, and CaO, which are mixed in a stoichiometric ratio. The ball milling medium is deionized water, the grinding speed is 120rpm, and the ball milling time is 8h. The pre-calcination temperature is 1200℃, and the temperature is kept for 3.5h.

[0044] S2: Add BaZrO3 and KTaO3 in the second ball milling, the grinding speed is 280rpm, and the ball milling time is 20h. Add polyvinyl alcohol solution during granulation, and add 0.06mL of 6% polyvinyl alcohol solution per gram of powder. Press the embryo body at a pressure of 50MPa, with a cylindrical diameter of 15mm and a height of 12mm. The embryo body debinding temperature is 500℃, and the temperature is kept for 1.5h. The sintering temperature is 1175℃, and the temperature is kept for 4.5h.

[0045] Example 5

[0046] A dielectric ceramic material, the chemical composition of which is: Ca m+l Ti mL i 2n Si n O (3m+3n+l) -yBaZrO3-zKTaO3; wherein x=0.84, y=0.12, z=0.04; m=0.91, n=0.05, l=0.04.

[0047] S1: The raw materials for the first ball milling are CaTiO3, Li2SiO3, and CaO, which are mixed in a stoichiometric ratio. The ball milling medium is deionized water, the grinding speed is 180rpm, and the ball milling time is 12h. The pre-calcination temperature is 1150℃, and the temperature is kept for 4h.

[0048] S2: Add BaZrO3 and KTaO3 in the second ball milling, the grinding speed is 240rpm, and the ball milling time is 18h. Add polyvinyl alcohol solution during granulation, and add 0.05mL of 6% polyvinyl alcohol solution per gram of powder. Press the embryo under 50MPa pressure, the cylinder diameter is 15mm, and the height is 12mm. The embryo debinding temperature is 450℃, and the temperature is kept for 1h. The sintering temperature is 1225℃, and the temperature is kept for 5h.

[0049] Example 6

[0050] A dielectric ceramic material, the chemical composition of which is: Ca m+l Ti mL i 2n Si n O(3m+3n+l) -yBaZrO3-zKTaO3; wherein x=0.79, y=0.19, z=0.02; m=0.86, n=0.10, l=0.04.

[0051] S1: The raw materials for the first ball milling are CaTiO3, Li2SiO3, and CaO, which are mixed in a stoichiometric ratio. The ball milling medium is deionized water, the grinding speed is 150rpm, and the ball milling time is 10h. The pre-calcination temperature is 1180℃, and the temperature is kept for 4.2h.

[0052] S2: BaZrO3 and KTaO3 were added in the second ball milling, the grinding speed was 260rpm, and the ball milling time was 19h. Polyvinyl alcohol solution was added during the granulation process, and 0.045mL of 6% polyvinyl alcohol solution was added per gram of powder. The pressing pressure of the embryo was 50MPa, the cylinder diameter was 15mm, and the height was 12mm. The embryo debinding temperature was 550℃, and the temperature was kept for 1.75h. The sintering temperature was 1200℃, and the temperature was kept for 4.25h.

[0053] Example 7

[0054] A dielectric ceramic material, the chemical composition of which is: Ca m+l Ti mL i 2n Si n O (3m+3n+l) -yBaZrO3-zKTaO3; wherein x=0.74, y=0.23, z=0.03; m=0.84, n=0.08, l=0.06.

[0055] S1: The raw materials for the first ball milling are CaTiO3, Li2SiO3, and CaO, which are mixed in a stoichiometric ratio. The ball milling medium is deionized water, the grinding speed is 140rpm, and the ball milling time is 9h. The pre-calcination temperature is 1170℃, and the temperature is kept for 3.8h.

[0056] S2: BaZrO3 and KTaO3 were added in the second ball milling, the grinding speed was 220rpm, and the ball milling time was 17h. Polyvinyl alcohol solution was added during the granulation process, and 0.055mL of 6% polyvinyl alcohol solution was added per gram of powder. The pressing pressure of the embryo was 50MPa, the cylinder diameter was 15mm, and the height was 12mm. The embryo debinding temperature was 480℃, and the temperature was kept for 1.25h. The sintering temperature was 1230℃, and the temperature was kept for 4.75h.

[0057] Example 8

[0058] A dielectric ceramic material, the chemical composition of which is: Ca m+l Ti mL i 2n Si n O (3m+3n+l)-yBaZrO3-zKTaO3; wherein x=0.81, y=0.17, z=0.02; m=0.92, n=0.05, l=0.03.

[0059] S1: The raw materials for the first ball milling are CaTiO3, Li2SiO3, and CaO, which are mixed in a stoichiometric ratio. The ball milling medium is deionized water, the grinding speed is 160rpm, and the ball milling time is 11h. The pre-calcination temperature is 1190℃, and the temperature is kept for 4.1h.

[0060] S2: BaZrO3 and KTaO3 were added in the second ball milling, the grinding speed was 270rpm, and the ball milling time was 19.5h. Polyvinyl alcohol solution was added during the granulation process, and 0.05mL of 6% polyvinyl alcohol solution was added per gram of powder. The pressing pressure of the embryo was 50MPa, the cylinder diameter was 15mm, and the height was 12mm. The embryo debinding temperature was 520℃, and the temperature was kept for 1.6h. The sintering temperature was 1240℃, and the temperature was kept for 4.9h.

[0061] Example 9

[0062] A dielectric ceramic material, the chemical composition of which is: Ca m+l Ti mL i 2n Si n O (3m+3n+l) -yBaZrO3-zKTaO3; wherein x=0.79, y=0.20, z=0.01; m=0.76, n=0.20, l=0.04.

[0063] S1: The raw materials for the first ball milling are CaTiO3, Li2SiO3, and CaO, which are mixed in a stoichiometric ratio. The ball milling medium is deionized water, the grinding speed is 130rpm, and the ball milling time is 9.5h. The pre-calcination temperature is 1160℃, and the temperature is kept for 3.9h.

[0064] S2: BaZrO3 and KTaO3 were added in the second ball milling, the grinding speed was 230rpm, and the ball milling time was 17.5h. Polyvinyl alcohol solution was added during the granulation process, and 0.058mL of 6% polyvinyl alcohol solution was added per gram of powder. The pressing pressure of the embryo was 50MPa, the cylinder diameter was 15mm, and the height was 12mm. The embryo debinding temperature was 580℃, and the temperature was kept for 1.8h. The sintering temperature was 1210℃, and the temperature was kept for 4.4h.

[0065] Example 10

[0066] A dielectric ceramic material, the chemical composition of which is: Ca m+l Ti mL i 2n Si n O (3m+3n+l)-yBaZrO3-zKTaO3; wherein x=0.85, y=0.13, z=0.02; m=0.80, n=0.15, l=0.05.

[0067] S1: The raw materials for the first ball milling are CaTiO3, Li2SiO3, and CaO, which are mixed in a stoichiometric ratio. The ball milling medium is deionized water, the grinding speed is 170rpm, and the ball milling time is 11.5h. The pre-calcination temperature is 1140℃, and the temperature is kept for 3.7h.

[0068] S2: BaZrO3 and KTaO3 were added in the second ball milling, the grinding speed was 250rpm, and the ball milling time was 18.5h. Polyvinyl alcohol solution was added during the granulation process, and 0.052mL of 6% polyvinyl alcohol solution was added per gram of powder. The pressing pressure of the embryo was 50MPa, the cylinder diameter was 15mm, and the height was 12mm. The embryo debinding temperature was 570℃, and the temperature was kept for 1.9h. The sintering temperature was 1220℃, and the temperature was kept for 4.6h.

[0069] Comparative Example 1: The same as Example 1, except that no polyvinyl alcohol solution was added during the granulation process.

[0070] Comparative Example 2: The same as Example 1, except that the concentration of the polyvinyl alcohol solution in step S2 is changed to 3%.

[0071] Comparative Example 3: The same as Example 1, except that: a dielectric ceramic material having a chemical composition of: Ca m+l Ti mL i 2n Si n O (3m+3n+l) -yBaZrO3-zKTaO3; wherein x=0.85, y=0.12, z=0.03; m=0.75, n=0.20, l=0.05" is replaced by "a dielectric ceramic material having a chemical composition of: Ca m+l Ti mL i 2n Si n O (3m+3n+l) -yBaZrO3-zKTaO3; wherein x=0.95, y=0.04, z=0.01; m=0.86, n=0.12, l=0.02".

[0072] Comparative Example 4: The same as Example 1, except that: a dielectric ceramic material having a chemical composition of: Ca m+l Ti mL i 2n Si n O (3m+3n+l)-yBaZrO3-zKTaO3; wherein x=0.85, y=0.12, z=0.03; m=0.75, n=0.20, l=0.05" is replaced by "a dielectric ceramic material having a chemical composition of: Ca m+l Ti mL i 2n Si n O (3m+3n+l) -yBaZrO3-zKTaO3; wherein x=0.70, y=0.25, z=0.05; m=0.70, n=0.27, l=0.03".

[0073] Comparative Example 5: The same as Example 1, except that: a dielectric ceramic material having a chemical composition of: Ca m+l Ti mL i 2n Si n O (3m+3n+l) -yBaZrO3-zKTaO3; wherein x=0.85, y=0.12, z=0.03; m=0.75, n=0.20, l=0.05" is replaced by "a dielectric ceramic material having a chemical composition of: Ca m+l Ti mL i 2n Si n O (3m+3n+l) -yBaZrO3-zKTaO3; wherein x=0.88, y=0.10, z=0.00; m=0.89, n=0.08, l=0.03".

[0074] Comparative Example 6: The same as Example 1, except that: a dielectric ceramic material having a chemical composition of: Ca m+l Ti mL i 2n Si n O (3m+3n+l) -yBaZrO3-zKTaO3; wherein x=0.85, y=0.12, z=0.03; m=0.75, n=0.20, l=0.05" is replaced by "a dielectric ceramic material having a chemical composition of: Ca m+l Ti mL i 2n Si n O (3m+3n+l) -yBaZrO3-zKTaO3; wherein x=0.85, y=0.12, z=0.03; m=0.80, n=0.15, l=0.05".

[0075] Comparative Example 7: The same as Example 1, except that: a dielectric ceramic material having a chemical composition of: Ca m+l TimL i 2n Si n O (3m+3n+l) -yBaZrO3-zKTaO3; wherein x=0.85, y=0.12, z=0.03; m=0.75, n=0.20, l=0.05" is replaced by a dielectric ceramic material, the chemical composition of which is: Ca m+l Ti mL i 2n Si n O (3m+3n+l) -yBaZrO3-zKTaO3; wherein x=0.92, y=0.07, z=0.01; m=0.71, n=0.24, l=0.05.

[0076] Comparative Example 8: The same as Example 1, except that: a dielectric ceramic material having a chemical composition of: Ca m+l Ti mL i 2n Si n O (3m+3n+l) -yBaZrO3-zKTaO3; wherein x=0.85, y=0.12, z=0.03; m=0.75, n=0.20, l=0.05" is replaced by "a dielectric ceramic material having a chemical composition of: Ca m+l Ti mL i 2n Si n O (3m+3n+l) -yBaZrO3-zKTaO3; wherein x=0.84, y=0.11, z=0.01; m=0.71, n=0.24, l=0.05".

[0077] Comparative Example 9: It is basically the same as Example 1, with the only difference being that: "After debinding, the heating rate of the smelting furnace is set to 3°C / min, the sintering temperature range is 1200°C, and after reaching the target temperature, it is kept warm for 4 hours" is replaced by "After debinding, the heating rate of the smelting furnace is set to 4°C / min, the sintering temperature range is 1200°C, and after reaching the target temperature, it is kept warm for 4 hours".

[0078] Comparative Example 10: It is basically the same as Example 1, with the only difference being that: "After debinding, the heating rate of the smelting furnace is set to 3°C / min, the sintering temperature range is 1200°C, and after reaching the target temperature, it is kept warm for 4 hours" is replaced by "After debinding, the heating rate of the smelting furnace is set to 5°C / min, the sintering temperature range is 1200°C, and after reaching the target temperature, it is kept warm for 4 hours".

[0079] Performance Testing

[0080] The dielectric ceramics prepared in the above-mentioned Examples 1 to 10 and Comparative Examples 1 to 6 were ground and polished to obtain ceramic finished products with a flat and smooth surface. The microwave dielectric properties of the cylindrical embryo ceramic at the resonant frequency were tested using a Keysight E5232B vector network analyzer as shown in Table 2:

[0081] Table 2

[0082]

[0083]

[0084] As shown in Table 2, the present invention uses titanate as the basis and adds lithium salt to prepare Ca m+l Ti mL i 2n Si n O (3m+3n+l) Precursor, adding BaZrO3 with high thermal conductivity and high stability, and then adding LiNbO3 with excellent dielectric properties. Through the synergistic effect between the components, the material performance is significantly improved, and a dielectric ceramic material with excellent microwave performance is prepared. Its relative dielectric constant ε r 9~11, Q×f(GHz)≥80000GHz, T f The range is -10~+10.8ppm / ℃, which has very high commercial application value and market prospects.

[0085] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A dielectric ceramic material, characterized in that: The preparation material of the dielectric ceramic material is Ca m+ l Ti mL i 2n Si n O (3m+3n+l) , BaZrO3, KTaO3, among which Ca m+l Ti mL i 2n Si n O (3m+3n+l) For the precursor.

2. A dielectric ceramic material according to claim 1, characterized in that: The chemical composition of the dielectric ceramic material is xCa m+l Ti mL i 2n Si n O (3m+3n+l) -yBaZrO3-zKTaO3; where x+y+z=1, x=0.75~0.92, y=0.05~0.20, z=0.03~0.06; Among them, m+n+l=1, m=0.72~0.85, n=0.12~0.25, l=0.01~0.

03.

3. A method for preparing a dielectric ceramic material according to any one of claims 1 to 2, characterized in that: The steps include: S1: Precursor Ca m+l Ti mL i 2n Si n O (3m+3n+l) Preparation: weigh raw materials CaTiO3, Li2SiO3, and CaO with a purity of more than 99.9% in proportion as the first grinding material, add zirconium oxide balls as grinding balls, add deionized water as ball milling media, perform the first ball milling, dry after the ball milling to obtain the first grinding material powder, pre-sinter the first grinding material, and cool to room temperature to obtain the precursor Ca m+l Ti mL i 2n Si n O (3m+3n+l) powder; S2: The precursor Ca prepared above m+l Ti mL i 2n Si n O (3m+3n+l) Powder and raw materials BaZrO3 and KTaO3 with a purity of more than 99.9% are used as the second grinding material, and are added into a ball mill in proportion for mixing, zirconium oxide spheres are added as grinding spheres, deionized water is added as ball milling media, and the second ball milling is carried out. After the ball milling is completed, the second grinding material powder is dried to obtain the second grinding material powder, and the second grinding material powder is granulated, pressed into an embryo, debinded, and sintered to obtain a dielectric ceramic material.

4. The method for preparing a dielectric ceramic material according to claim 3, characterized in that: The grinding speed of the first ball milling is 120-180 rpm, and the ball milling time is 8-12 hours; the weight ratio of the first grinding material, zirconium oxide spheres, and deionized water is 1:2:

2.

5. The method for preparing a dielectric ceramic material according to claim 3, characterized in that: The pre-burning temperature rise rate is 5°C / min, the pre-burning temperature range is 1100°C to 1200°C, and after reaching the target temperature, the temperature is kept for 3.5 to 4.5 hours.

6. The method for preparing a dielectric ceramic material according to claim 3, characterized in that: The grinding speed of the second ball milling is 200-280 rpm, and the ball milling time is 16-20 hours; the weight ratio of the second grinding material, zirconium oxide spheres, and deionized water is 1:2:1.

5.

7. The method for preparing a dielectric ceramic material according to claim 3, characterized in that: The specific process of the granulation treatment is to add a poly(ethylene glycol) solution as a binder to the second grinding material powder, add 0.04-0.06 mL of a 6% poly(ethylene glycol) solution per gram of powder, mix well, and then granulate to obtain granulated powder.

8. The method for preparing a dielectric ceramic material according to claim 3, characterized in that: The pressed embryo body is a cylindrical embryo body with a diameter of 15 mm and a height of 12 mm, which is formed by pressing the granulated powder under a pressure of 50 MPa.

9. A method for preparing a dielectric ceramic material according to claim 8, characterized in that: The debinding of the embryo body is to place the cylindrical embryo body into a smelting furnace, set the heating rate of the smelting furnace to 5°C / min, the debinding temperature range to 400°C to 600°C, and keep the temperature for 1 to 2 hours after reaching the target temperature.

10. The method for preparing a dielectric ceramic material according to claim 3, characterized in that: The sintering is to set the heating rate of the smelting furnace to 3°C / min after debinding, and the sintering temperature range is 1150°C to 1250°C. After reaching the target temperature, the temperature is kept for 3.5 to 5 hours.

Citation Information

Patent Citations

  • Low-temperature sintering microwave medium material with C0G characteristics and preparing method thereof

    CN104341144A

  • Microwave ceramic material and preparation method thereof

    CN107266074A

  • Composite microwave dielectric ceramic material and preparation method thereof

    CN113321496A

  • Low-temperature sintered microwave dielectric ceramic and preparation method thereof

    CN114988860A

  • Dielectric ceramic material with high energy storage performance and negative capacitance temperature coefficient and preparation