Pressureless sintering hexagonal boron nitride ceramic and preparation method thereof

Through the pressure-free sintering process, h-BN and h-BNw are mixed and sintered in a specific proportion, which solves the problems of high cost and low efficiency of the hot press sintering process, and realizes the stability and high strength of hexagonal boron nitride ceramics, satisfying the satisfaction of Industrialization needs.

CN118908736APending Publication Date: 2024-11-08SHANDONG JINGYI NEW MATERIALS CO LTD +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411120121.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing hot press sintering process of hexagonal boron nitride ceramics has problems such as expensive equipment, high energy consumption and low production efficiency, which limits its industrialization development, and composite ceramics are difficult to meet the needs of pure h-BN ceramics.

Method used

By using the pressure-free sintering process, by mixing h-BN and h-BNw in a specific proportion, after stirring, drying, crushing, adding binder and pressing into thin sheets, it is sintered under NH3 atmosphere to form an apparent density of 1.30. g/cm3~2.00g/cm3, pressure-free sintered hexagonal boron nitride ceramic with a bending strength of 15MPa~20MPa.

Benefits of technology

The stability and singularity of the ceramic phase are achieved, the equipment cost is reduced, the requirements of h-BN crucibles and high-temperature resistant plates are met, and the density and bending strength of h-BN ceramics are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908736A_ABST
    Figure CN118908736A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of ceramic materials, and relates to pressureless sintering hexagonal boron nitride ceramic and a preparation method thereof, the chemical general formula of the hexagonal boron nitride ceramic is (1-x) h-BN + xh-BNw, x is more than or equal to 0.1 and less than or equal to 0.8, and h-BNw represents hexagonal boron nitride whiskers; the apparent density rho ap is 1.30 g / cm < 3 > to 2.00 g / cm < 3 >, and the bending strength sigma b is 15 MPa to 20 MPa. The ceramic prepared by the invention is stable and single in phase, and can meet the requirements of h-BN crucibles and high-temperature-resistant plates; in the preparation process, the stoichiometric ratio is accurately controlled, the process is simple, the cost of used equipment is low, and various requirements of preparation of the h-BN ceramic special-shaped part can be met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of ceramic materials, and in particular relates to a pressureless sintered hexagonal boron nitride ceramic and a preparation method thereof. Background Art

[0002] Hexagonal boron nitride (h-BN) ceramic materials have broad application prospects in magnetohydrodynamic launch devices, plasma jet furnaces, crucibles, boats, high-frequency electrical insulation materials, integrated circuit heat sinks and ion rocket nozzles due to their excellent thermal shock resistance, corrosion resistance, electrical insulation, lubricity and machinability. At present, the preparation of h-BN ceramics usually adopts the hot pressing sintering process, which can significantly improve the density of ceramics. However, the hot pressing sintering process has the disadvantages of expensive large hot pressing equipment, high energy consumption during use, and limited production efficiency. This series of problems has caused the high cost of h-BN ceramics, further limiting the development of h-BN ceramics industrialization. Therefore, the development of pressureless sintering process for h-BN ceramics is helpful to solve various problems that need to be solved urgently in the process of industrialization.

[0003] In recent years, the research on the pressureless sintering process of h-BN ceramics can be roughly divided into three categories. The first is to improve the size of h-BN sheets by hot pressing (spark plasma) sintering. For example, 2μm size h-BN sheets can be sintered at 1800℃ / 30MPa to obtain σ b =53MPa; the second is reaction sintering, which also uses hot pressing sintering process, for example, h-BN+B is sintered at 1850℃ / 0.2MPa in N2 atmosphere. b =45MPa; the third is to add oxide sintering aids, still using hot pressing sintering process, for example, 80wt.%BN+20wt.%(La2O3-Al2O3) sintered at 1900℃ / 30MPa can obtain 133MPa bending strength; however, hot pressing sintering has always been a key issue restricting the development of its related industries, and composite ceramics often cannot meet the demand for pure h-BN ceramics in related fields. Therefore, the use of h-BN and h-BN w The development and production of pressureless sintering process after mixing is of great significance to the development of h-BN ceramic industry. Summary of the invention

[0004] In view of the deficiencies of the above-mentioned prior art, the present invention provides a pressureless sintered hexagonal boron nitride ceramic and a preparation method thereof. The specific technical scheme is as follows: The first object of the present invention is to provide a pressureless sintered hexagonal boron nitride ceramic, the chemical formula of which is: (1-x)h-BN+xh-BN w , where 0.1≤x≤0.8, h-BN w represents hexagonal boron nitride whiskers; apparent density (ρap ) is 1.30g / cm 3 ~2.00g / cm 3 , flexural strength (σ b ) is 15MPa~20MPa.

[0005] The ceramic phase of the present invention is stable and single, and can meet the requirements of h-BN crucible and high temperature resistant plate.

[0006] The second object of the present invention is to provide a method for preparing the above-mentioned pressureless sintered hexagonal boron nitride ceramic, comprising the following steps: (1) Ingredients: h-BN and h-BN w The raw materials are formulated according to the chemical formula; (2) Mixing: The ingredients in step (1) are stirred and mixed with deionized water to obtain a slurry, and the slurry is dried; (3) Grinding and screening: grinding and screening the slurry dried in step (2) to obtain a sieved powder; (4) Adding a binder: adding the sieved powder in step (3) to the binder, heating, stirring and mixing evenly, and then sieving to obtain a binder powder; (5) Pressing: The powder with binder added in step (4) is pressed into a thin sheet with a thickness of 1 to 3 mm through a grinding tool and a tablet press; (6) Sintering: Sinter the green sheet obtained in step (5) in an NH3 atmosphere.

[0007] The h-BN ceramic of the present invention is prepared with boron nitride flakes and whiskers as raw materials, wherein the whiskers are recrystallized at high temperature to generate small-sized boron nitride flakes that can fill the pores of the h-BN ceramic, enhance its compactness, and further enhance its strength. The preparation process of the present invention has precise stoichiometric ratio control, simple process, low equipment cost, and the prepared h-BN ceramic can meet various requirements for the preparation of h-BN ceramic special-shaped parts.

[0008] Furthermore, the h-BN raw material is h-BN powder with a purity of 99.9% and a microscopic sheet size of 3-30 μm; preferably, the microscopic sheet size is 8 μm; w The raw material is h-BN with a purity of 99.0% and a microscopic size of 1-10μm in width and 1-100μm in length. w Block.

[0009] Furthermore, in step (2), the ratio of powder to deionized water is 50 g: (50-1000) ml; and the stirring speed is 100-400 r / min.

[0010] Furthermore, in step (2), the drying temperature is 50°C to 100°C, and the drying time is 1 to 24 hours.

[0011] Furthermore, in step (3) and step (4), screening is performed through a standard sieve of 40 to 300 meshes.

[0012] Furthermore, in step (4), the binder is paraffin wax, the amount of the paraffin wax is 2-20 wt.% of the sieved powder, and the heating and mixing temperature is 120°C-200°C.

[0013] Furthermore, in step (5), the tablet press applies a unidirectional pressure of 2 to 20 t.

[0014] Furthermore, in step (6), the sintering temperature is 1500° C. to 2000° C., the holding time is 1 to 24 h, and the NH3 ventilation rate is 10 to 80 ml / min.

[0015] The beneficial effects of the present invention are: The ceramic phase prepared by the present invention is stable and single, and can meet the requirements of h-BN crucibles and high-temperature resistant plates; the stoichiometric ratio is accurately controlled during preparation, the process is simple, the equipment cost is low, and the repeatability is good, which can meet various requirements for the preparation of h-BN ceramic special-shaped parts. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 This is a SEM image of the ceramic prepared in Example 1 of the present invention.

[0017] Figure 2 This is the SEM image of the ceramic prepared in Example 2 of the present invention.

[0018] Figure 3 This is a SEM image of the ceramic prepared in Example 3 of the present invention. DETAILED DESCRIPTION

[0019] The principles and features of the present invention are described below in conjunction with embodiments. The examples given are only used to explain the present invention and are not used to limit the scope of the present invention.

[0020] Example 1 Preparation of 70wt.%h-BN+30wt.%h-BNw ceramics: (1) Ingredients: 70g of h-BN powder with a purity greater than 99.9% and a size of about 8μm and block h-BN with a purity greater than 99.0% and a size of about 3μm wide and 10μm long were mixed. w 30g of raw material is accurately weighed; (2) Mixing: Mix 70g h-BN and 30g h-BN weighed in step (1) wThe raw materials and 800 ml of deionized water were added to a 1000 ml beaker, and stirred at 350 r / min for 12 h using a mechanical stirrer, with the stirring head 2 cm to 3 cm from the bottom of the beaker; the mixed slurry was transferred to a glass evaporating dish, and then placed in a forced air drying oven at 80 ° C for 24 h; (3) Crushing and screening: the powder dried in step (2) is ground in an Al2O3 mortar and then sieved through an 80-mesh standard sieve; (4) Adding a binder: weigh the powder sieved in step (3) and add 5.0% of the powder mass of paraffin particles as a binder, heat at 150° C., stir and mix evenly, and sieve the powder after adding the binder through an 80-mesh standard sieve; (5) Pressing: The powder after adding the binder in step (4) is pressed 10 tons in one direction by a manual hydraulic press to press the powder into a 40 mm*40 mm thin sheet with a thickness of about 2 mm. w Greenware; (6) Sintering: The green body pressed in step (5) was sintered at 1800°C for 4 h in an atmosphere of NH3 with a flow rate of 40 ml / min to form h-BN ceramics, and 70 wt.% h-BN + 30 wt.% h-BN was obtained. w ceramics.

[0021] from Figure 1 It can be seen from the SEM of Example 1 that the prepared h-BN ceramic is composed of boron nitride sheets with a single structure. The boron nitride sheets are stacked and arranged in a relatively orderly manner. There are some small-sized boron nitride sheets, which is the result of h-BN at high temperature. w It is transformed by recrystallization, which is beneficial to improve the density and flexural strength of h-BN ceramics.

[0022] Example 2 Preparation of 60wt.%h-BN+40wt.%h-BNw ceramics: (1) Ingredients: 60g of h-BN powder with a purity greater than 99.9% and a size of about 8μm and block h-BN with a purity greater than 99.0% and a size of about 3μm wide and 10μm long are mixed. w 40g of raw material is accurately weighed; (2) Mixing: Mix 60g h-BN and 40g gh-BN weighed in step (1) w The block and 800 ml of deionized water were added to a 1000 ml beaker and stirred at 350 r / min for 12 h with a mechanical stirrer, with the stirring head 2 cm to 3 cm from the bottom of the beaker. The mixed slurry was transferred to a glass evaporating dish and then dried in a forced air drying oven at 80 °C for 24 h. (3) Crushing and screening: the powder dried in step (2) is ground in an Al2O3 mortar and then sieved through an 80-mesh standard sieve; (4) Adding a binder: weigh the powder sieved in step (3) and add 5.0% of the powder mass of paraffin particles as a binder, heat at 150° C., stir and mix evenly, and sieve the powder after adding the binder through an 80-mesh standard sieve; (5) Pressing: The powder after adding the binder in step (4) is pressed 10 tons in one direction by a manual hydraulic press to press the powder into a 40 mm*40 mm thin sheet with a thickness of about 2 mm. w Greenware; (6) Sintering: The green body pressed in step (5) was sintered at 1800°C for 4 h in an atmosphere of NH3 with a flow rate of 40 ml / min to form h-BN ceramics, and the obtained 60 wt.% h-BN + 40 wt.% h-BN w ceramics.

[0023] from Figure 2 It can be seen from the SEM of Example 2 that the prepared h-BN ceramic is composed of randomly arranged boron nitride sheets, and the phase is stable and single. Figure 2 It can be seen that many small-sized boron nitride flakes are scattered between the large-sized boron nitride flakes. These small-sized boron nitride flakes are h-BN w The product is recrystallized at high temperature, which fills the pores between large-sized boron nitride sheets, making the prepared boron nitride ceramics denser and improving its flexural strength.

[0024] Example 3 50wt.%h-BN+50wt.%h-BN w Preparation of ceramics: (1) Ingredients: 50 g of h-BN powder with a purity greater than 99.9% and a size of about 8 μm and a block of h-BN with a purity greater than 99.0% and a size of about 3 μm wide and 10 μm long were mixed. w 50g of raw material is accurately weighed; (2) Mixing: Mix the 50gh-BN and 50gh-BN weighed in step (1) w and 800 ml of deionized water were added into a 1000 ml beaker, and stirred at 350 r / min for 12 h using a mechanical stirrer, with the stirring head 2 cm to 3 cm away from the bottom of the beaker; the mixed slurry was transferred into a glass evaporating dish, and then placed in a forced air drying oven at 80 ° C for drying for 24 h; (3) Crushing and screening: the powder dried in step (2) is ground in an Al2O3 mortar and then sieved through an 80-mesh standard sieve; (4) Adding a binder: weigh the powder sieved in step (3) and add 5.0% of the powder mass of paraffin particles as a binder, heat at 150° C., stir and mix evenly, and sieve the powder after adding the binder through an 80-mesh standard sieve; (5) Pressing: The powder after adding the binder in step (4) is pressed 10 tons in one direction by a manual hydraulic press to press the powder into a 40 mm*40 mm thin sheet with a thickness of about 2 mm. w Greenware; (6) Sintering: The green body pressed in step (5) was sintered at 1800°C for 4 h in an atmosphere of NH3 with a flow rate of 40 ml / min to form h-BN ceramics, and the obtained 50 wt.% h-BN + 50 wt.% h-BN w ceramics.

[0025] from Figure 3 It can be seen from the SEM of Example 3 that the prepared h-BN ceramics are mainly composed of boron nitride sheets, among which the small-sized boron nitride sheets are composed of h-BN w Recrystallization forms, they fill in the space between large-sized boron nitride sheets, enhance the density of h-BN ceramics, and are beneficial to the improvement of their flexural strength.

[0026] The relevant process parameters of Examples 1 to 3 and the apparent density and flexural strength properties of the obtained ceramics are shown in Table 1.

[0027] Table 1 Relevant process parameters of Examples 1 to 3 and apparent density and flexural strength performance of the obtained ceramics It can be seen from the data in Table 1 that with the increase of h-BNw content, the flexural strength of the prepared boron nitride ceramic first increases and then decreases. When the h-BNw mass content is 40%, the flexural strength of the boron nitride ceramic reaches the maximum, which is 17.2MPa, and the performance is excellent. It can be seen from the SEM images of the comparative examples that the h-BN ceramic prepared by the present invention is composed of h-BN sheets, wherein h-BN w The small-sized boron nitride flakes formed by recrystallization fill the pores between the large-sized h-BN flakes, which can effectively enhance the density and bending resistance of h-BN ceramics. w When the content is low, the h-BN ceramics have more pores, while the h-BN w When the content is high, h-BN ceramics will contain h-BN w Residue, which will reduce the bending strength of h-BN ceramics.

[0028] The h-BN ceramics prepared by the present invention can meet the requirements of h-BN crucibles and high temperature resistant plates; during the preparation, the stoichiometric ratio is accurately controlled, the process is simple, the equipment cost is low, and various requirements for the preparation of h-BN ceramic special-shaped parts can be met.

[0029] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A pressureless sintered hexagonal boron nitride ceramic, characterized in that: The general chemical formula is: (1-x)h-BN+xh-BN w , where 0.1≤x≤0.8, h-BN w represents hexagonal boron nitride whisker; apparent density ρ ap 1.30g / cm 3 ~2.00g / cm 3 , flexural strength σ b It is 15MPa~20MPa.

2. A method for preparing the pressureless sintered hexagonal boron nitride ceramic according to claim 1, characterized in that: The steps include: (1) Ingredients: h-BN and h-BN w The raw materials are formulated according to the chemical formula; (2) Mixing: The ingredients in step (1) are stirred and mixed with deionized water to obtain a slurry, and the slurry is dried; (3) Grinding and screening: grinding and screening the slurry dried in step (2) to obtain a sieved powder; (4) Adding a binder: adding the sieved powder in step (3) to the binder, heating, stirring and mixing evenly, and then sieving to obtain a binder powder; (5) Pressing: The powder with the binder added in step (4) is pressed into a thin sheet-like green body through a grinding tool and a tablet press; (6) Sintering: The green sheet obtained in step (5) is sintered in an NH3 atmosphere.

3. The method for preparing the pressureless sintered hexagonal boron nitride ceramic according to claim 2, characterized in that: The h-BN raw material is h-BN powder with a purity of 99.9% and a microscopic sheet size of 3-30 μm; w The raw material is h-BN with a purity of 99.0% and a microscopic size of 1-10μm in width and 1-100μm in length. w Block.

4. The method for preparing the pressureless sintered hexagonal boron nitride ceramic according to claim 2, characterized in that: In the step (2), the ratio of powder to deionized water is 50 g: (50-1000) ml; the stirring speed is 100-400 r / min.

5. The method for preparing pressureless sintered hexagonal boron nitride ceramics according to claim 2, characterized in that: In the step (2), the drying temperature is 50°C to 100°C, and the drying time is 1 to 24 hours.

6. The method for preparing pressureless sintered hexagonal boron nitride ceramics according to claim 2, characterized in that: In the steps (3) and (4), screening is performed through a standard sieve of 40 to 300 meshes.

7. The method for preparing pressureless sintered hexagonal boron nitride ceramics according to claim 2, characterized in that: In the step (4), the binder is paraffin wax, the amount of the paraffin wax is 2-20 wt.% of the sieved powder, and the heating and mixing temperature is 120°C-200°C.

8. The method for preparing pressureless sintered hexagonal boron nitride ceramics according to claim 2, characterized in that: In the step (5), the tablet press applies a unidirectional pressure of 2 to 20 tons.

9. The method for preparing pressureless sintered hexagonal boron nitride ceramics according to claim 2, characterized in that: The sintering temperature in step (6) is 1500° C. to 2000° C., the holding time is 1 to 24 h, and the NH3 ventilation rate is 10 to 80 ml / min.

Citation Information

Patent Citations

  • Method for preparing high-purity hexagonal boron nitride ceramic by pressureless sintering

    CN104193341A

  • Preparation method of boron nitride fiber enhanced nitride ceramic-based composite material

    CN106986658A

  • Hexagonal boron nitride sintered compact

    JP2001328868A

  • Pressureless sintered body of boron nitride

    US5063184A