Continuous carbon fiber reinforced ultra-high temperature ceramic matrix composite material and preparation method thereof
By employing slurry injection and precursor impregnation pyrolysis processes, the problems of long preparation cycles and high costs of continuous carbon fiber reinforced ultra-high temperature ceramic matrix composites have been solved, enabling rapid and low-cost preparation of ceramic matrix composites and improving the densification and ablation resistance of the materials.
Patent Information
- Application Number
- CN202410845260.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-11-08
AI Technical Summary
In existing technologies, the preparation cycle of continuous carbon fiber reinforced ultra-high temperature ceramic matrix composites is long, the cost is high, and the densification effect is poor, making it difficult to meet the thermal protection material requirements of hypersonic vehicles.
By employing a slurry injection combined with precursor impregnation and pyrolysis process, ceramic slurry is introduced into the fiber preform and cured and pyrolyzed. This is combined with vacuum impregnation and pressure impregnation to achieve uniform distribution and densification of the ceramic matrix.
It enables rapid preparation of composite materials with complete fiber structure and uniform component distribution, reduces preparation cost, and improves the densification degree and anti-oxidation and ablation performance of the material.
Smart Images

Figure CN118908741A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of composite material preparation, for example, to a continuous carbon fiber reinforced ultra-high temperature ceramic matrix composite material and a preparation method thereof, the main function of which is to achieve rapid and low-cost preparation of continuous carbon fiber reinforced ultra-high temperature ceramic matrix composite materials. Background Art
[0002] At present, hypersonic aircraft have become a flight equipment that is being developed in competition in related fields. With the continuous increase in flight speed, the service environment of hypersonic aircraft has put forward more stringent requirements on its thermal protection materials, including oxidation resistance, ablation resistance, long service life and structural integrity. At the same time, continuous carbon fiber reinforced ultra-high temperature ceramic matrix composites have excellent properties such as low density, high strength, high temperature resistance and oxidation and ablation resistance while overcoming the intrinsic brittleness of ceramics. It is currently the most promising new generation of thermal protection materials.
[0003] In the related art, document 1 "Preparation and properties of C / TaC composite svia PIP process" shows that the preparation of C / TaC composite materials using the PIP process requires at least 15 cycles of impregnation and cracking, and the preparation cycle is 17 to 20 days. The various chemical reactions that occur in the precursor polymer during the cracking process are relatively complex, and it is difficult to accurately control the cracking products and their content. Because of its high reactivity, when the precursor polymer is directly introduced into the carbon fiber preform, it is very easy to react with the carbon fiber to cause structural damage, resulting in a decrease in the toughening effect of the fiber. The composite materials prepared by the PIP process have uniform distribution of components, but the high cost of the precursor and the long manufacturing cycle are the main disadvantages of this process.
[0004] In addition, document 2 "Fabrication and mechanical properties of 3-D Cf / C-SiC-TiC composites prepared by RMI" shows that the composite materials prepared by the RMI melt infiltration process need to introduce an appropriate amount of matrix inside the carbon fiber preform to protect the erosion of the fiber by the molten alloy during the melt infiltration process. The prepared composite materials have the characteristics of fast densification speed and high density, but the fiber structure will inevitably be damaged to a certain extent during the high-temperature reaction melt infiltration process.
[0005] At the same time, Chinese patent CN112341228B discloses a C / ZrC-SiC ultra-high temperature ceramic-based composite material and a preparation method thereof. The method is as follows: preparing a powdered carbon fiber preform formed by alternatingly stacking carbon cloth layers and ZrC powder layers; preparing a C interface layer on the surface of the powdered carbon fiber preform to obtain a low-density C / C composite material; using a polycarbosilane precursor solution as an impregnation liquid to densify the SiC matrix of the low-density C / C composite material through a PIP process; repeating the PIP process multiple times to obtain a C / ZrC-SiC ultra-high temperature ceramic-based composite material. The method of the present invention has strong process applicability, simple preparation process, and easy operation. The amount of ZrC powder added in the obtained C / ZrC-SiC ultra-high temperature ceramic-based composite material is adjustable and controllable, and has excellent mechanical properties and antioxidant and ablation resistance, and has broad application prospects in the field of aerospace.
[0006] In addition, Chinese patent CN112457020B discloses a multifunctional ultra-high temperature ceramic-based composite material and a preparation method thereof. The method is as follows: (1) burying one end of a porous carbon / carbon intermediate in zirconium-silicon alloy powder, and performing a melt infiltration reaction at high temperature to obtain a ZrC / SiC matrix; (2) impregnating the other end of the porous carbon / carbon intermediate after step (1) with a hafnium-silicon integrated ceramic precursor solution, and then sequentially performing the steps of curing and high-temperature cracking to obtain an ultra-high temperature ceramic matrix composed of a ZrC / SiC matrix and a HfC / SiC matrix; (3) depositing a SiC sealing layer on the surface of the ultra-high temperature ceramic matrix by chemical vapor deposition to obtain a multifunctional ultra-high temperature ceramic-based composite material. The multifunctional ultra-high temperature ceramic-based composite material prepared by the present invention comprises a dense ZrC / SiC matrix, which can improve the high-temperature air tightness of the composite material; and a uniformly distributed HfC / SiC matrix, which can improve the high-temperature ablation resistance of the composite material.
[0007] In the process of implementing the embodiments of the present disclosure, it was found that the composite processes such as slurry impregnation + precursor impregnation cracking method in the related art have technical problems such as long preparation cycle, high cost, poor densification effect, etc., which limit its actual engineering application. Therefore, developing a new carbon fiber reinforced ultra-high temperature ceramic matrix composite process has become a key issue in this direction.
[0008] It should be noted that the information disclosed in the above background technology section is only used to enhance the understanding of the background of the present application, and therefore may include information that does not constitute the prior art known to ordinary technicians in the field. Summary of the invention
[0009] In order to provide a basic understanding of some aspects of the disclosed embodiments, a brief summary is given below. The summary is not an extensive review, nor is it intended to identify key / critical components or delineate the scope of protection of these embodiments, but rather serves as a prelude to the detailed description that follows.
[0010] The disclosed embodiment provides a continuous carbon fiber reinforced ultra-high temperature ceramic matrix composite material and its preparation method, which combines slurry injection and slurry impregnation processes to achieve rapid and uniform introduction of ceramic components during material preparation, and then densification is achieved through precursor impregnation cracking to obtain a carbon fiber reinforced ceramic matrix composite material. The invention can obtain a well-densified carbon fiber reinforced ceramic matrix composite material, in order to solve the problems of long preparation cycle, high cost and poor densification effect existing in the current precursor impregnation cracking, and lay an industrial foundation for the rapid preparation of composite materials.
[0011] In some embodiments, a method for preparing a continuous carbon fiber reinforced ultra-high temperature ceramic matrix composite material is provided to reduce the cost of the ceramic matrix composite material preparation process and make up for the shortcomings of the existing process, including:
[0012] S1: mixing a solvent, a dispersant and a ceramic powder to prepare a ceramic slurry;
[0013] S2: depositing an interface inside the fiber braid to prepare a fiber preform;
[0014] S3: Injecting the ceramic slurry in step S1 into the central area of the fiber preform in step S2, followed by curing and cracking to prepare a first intermediate;
[0015] S4: introducing the ceramic slurry in step S1 into the edge area of the fiber preform in step S2 except the central area by vacuum impregnation and pressure impregnation, and then curing and cracking to prepare a second intermediate;
[0016] S5: Densification by Precursor Impregnation Pyrolysis (PIP) process, whereby the precursor polymer solution is introduced into the second intermediate by impregnation, followed by curing and pyrolysis to convert the second intermediate into a silicon carbide ceramic component, thereby obtaining a densified continuous carbon fiber reinforced ultrahigh temperature ceramic matrix composite material.
[0017] Optionally, in step S1, the solvent is a first type solvent or a second type solvent, the first type solvent includes one or more of deionized water, anhydrous ethanol, acetone, xylene, and toluene; the second type solvent includes one or more of polycarbosilane (PCS), polysilazane, polyborazane, and polysiloxane; the dispersant includes one or more of trioctylphosphine oxide (TOPO), carboxymethyl cellulose (CMC), polyacrylamide (PAM), and polyvinyl alcohol (PVA).
[0018] Optionally, in step S1, the ceramic powder is a boride, a carbide or a nitride; the content of the ceramic powder in the ceramic slurry is 5 to 90 wt%; the content of the dispersant in the ceramic slurry is 0.5 to 10% of the mass of the ceramic powder; and the particle size of the ceramic powder is 0.05 to 50 μm.
[0019] Optionally, in step S1, the fiber preform includes carbon fiber, SiC fiber, silicon nitride fiber, glass fiber or oxide fiber; the molding method of the fiber preform includes two-dimensional lamination, three-dimensional needle-punched fiber or three-dimensional weaving; the fiber content of the fiber preform is 10-75 vol%.
[0020] Optionally, in step S2, the material of the interface includes one or more of pyrolytic carbon PyC, boron nitride BN, silicon carbide SiC, and silicon nitride Si3N4; and the deposition thickness of the interface is 50 to 600 nm.
[0021] Optionally, in step S3, the ceramic slurry is arranged in a lattice in the central area of the fiber preform, and the form of the injection lattice includes a circular arrangement, a rectangular arrangement or an irregular arrangement; in step S3, the curing and cracking processes are both carried out in an inert gas, wherein the curing temperature is 80 to 400°C, and the insulation time is 0.5 to 3 hours; the cracking temperature is 600 to 1400°C, and the insulation time is 0.5 to 3 hours.
[0022] Optionally, in step S3, during injection, the injection spacing along three mutually perpendicular directions is 2 to 10 mm, the inner diameter of the needle used for injection is 0.2 to 1 mm, the injection time of the injection array is 0.5 to 2.0 s, and the injection pressure is 0.5 to 1.5 MPa.
[0023] Optionally, in step S4, the vacuum impregnation and pressure impregnation include: first placing the first intermediate in an environment with a vacuum degree lower than -0.09 MPa for standing, and then placing it in the ceramic slurry in step S1 for pressure impregnation, wherein the pressure of the pressure impregnation is 0.5 to 3 MPa, and the pressure impregnation time is 0.5 to 2 hours; in step S4, the curing and cracking process is carried out in an inert gas, wherein the curing temperature is 80 to 400°C, the insulation time is 0.5 to 3 hours, and the cracking temperature is 600 to 1400°C, and the insulation time is 0.5 to 3 hours.
[0024] Optionally, in step S5, the precursor polymer includes one or more of polycarbosilane, polysilazane, polyborazane, and polysiloxane; in step S5, the impregnation includes vacuum impregnation and pressure impregnation, and the vacuum impregnation and pressure impregnation include: first placing the first intermediate in an environment with a vacuum degree lower than -0.09 MPa for standing, and then placing it in a precursor polymer solution for pressure impregnation, wherein the pressure of the pressure impregnation is 0.5 to 3 MPa, and the pressure impregnation time is 0.5 to 2 hours; in step S5, the curing and cracking processes are both carried out in an inert gas, wherein the curing temperature is 80 to 400°C, the insulation time is 0.5 to 4 hours, and the cracking temperature is 600 to 1400°C, and the insulation time is 0.5 to 3 hours.
[0025] In some embodiments, a continuous carbon fiber reinforced ultra-high temperature ceramic matrix composite material prepared by the preparation method of the present application is provided.
[0026] The present application provides a method for preparing a continuous carbon fiber reinforced ultra-high temperature ceramic matrix composite material C by combining slurry injection with precursor impregnation pyrolysis. f / UHTCs-SiC process can achieve the following technical effects:
[0027] The present application provides a process method for preparing continuous carbon fiber reinforced ultra-high temperature ceramic matrix composite material Cf / UHTCs-SiC by combining slurry injection with precursor impregnation and pyrolysis. After the fiber braid is deposited through the interface layer, the ceramic powder can be introduced into the central area of the fiber preform by injection process, and then the ceramic powder is introduced into the edge area of the fiber preform by slurry impregnation to achieve uniform distribution of the ceramic matrix in the preform. Finally, the precursor impregnation and pyrolysis process is used for densification. In this way, the present application has the advantages of short cycle, uniform distribution of components, and complete fiber structure. In addition, the present application protects the structural integrity of the fiber during the preparation process, improves the uniform distribution of components inside the material, and can greatly shorten the preparation cycle of the composite material to meet industry needs.
[0028] The above general description and the following description are exemplary and explanatory only and are not intended to limit the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] One or more embodiments are exemplarily described by corresponding drawings, which do not limit the embodiments. Elements with the same reference numerals in the drawings are shown as similar elements, and the drawings do not constitute a scale limitation, and wherein:
[0030] Figure 1 This is a flow chart of a method for preparing a continuous carbon fiber reinforced ultra-high temperature ceramic matrix composite material provided by the present application;
[0031] Figure 2 This application provides a C f / UHTCs-SiC composite material preparation flow chart;
[0032] Figure 3 This is a porous C prepared by slurry injection in Example 1 provided in this application. f CT images of / ZrB2-SiC composite materials: (a) 3D reconstruction model; (b) XY plane ray image;
[0033] Figure 4 C of Example 1 of the present application f Microscopic morphology of ZrB2-SiC composites: (a) web layer area; (b) fiber bundle area;
[0034] Figure 5 is C of Example 1 provided in this application f Schematic diagram of the three-dimensional morphology of the surface of / ZrB2-SiC composite material before and after ablation. DETAILED DESCRIPTION
[0035] In order to be able to understand the features and technical contents of the embodiments of the present disclosure in more detail, the implementation of the embodiments of the present disclosure is described in detail below in conjunction with the accompanying drawings. The attached drawings are for reference only and are not used to limit the embodiments of the present disclosure. In the following technical description, for the convenience of explanation, a full understanding of the disclosed embodiments is provided through multiple details. However, one or more embodiments can still be implemented without these details. In other cases, to simplify the drawings, well-known structures and devices can be simplified for display.
[0036] The terms "first", "second", etc. in the specification and claims of the embodiments of the present disclosure and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the terms used in this way can be interchanged where appropriate, so as to describe the embodiments of the embodiments of the present disclosure described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions.
[0037] Unless otherwise stated, the term "plurality" means two or more.
[0038] In the embodiment of the present disclosure, the character " / " indicates that the preceding and following objects are in an "or" relationship. For example, A / B indicates: A or B.
[0039] The term "and / or" is a description of the association relationship between objects, indicating that three relationships can exist. For example, A and / or B means: A or B, or, A and B.
[0040] The term "correspondence" may refer to an association relationship or a binding relationship. The correspondence between A and B means that there is an association relationship or a binding relationship between A and B.
[0041] The experimental methods and detection methods in the following embodiments are conventional methods unless otherwise specified; the reagents and materials are commercially available unless otherwise specified.
[0042] In the related art, document 1 "Preparation and properties of C / TaC composites via PIP process" shows that the preparation of C / TaC composites by PIP process requires at least 15 cycles of impregnation and cracking, and the preparation cycle is 17 to 20 days. The various chemical reactions that occur in the precursor polymer during the cracking process are relatively complex, and it is difficult to accurately control the cracking products and content. Because of its high reactivity, when the precursor polymer is directly introduced into the carbon fiber preform, it is very easy to react with the carbon fiber to cause structural damage, resulting in a decrease in the toughening effect of the fiber. The composite material prepared by the PIP process has a uniform distribution of components, but the high cost of the precursor and the long manufacturing cycle are the main disadvantages of this process.
[0043] In addition, the literature 2 “Fabrication and mechanical properties of 3-DC f / C-SiC-TiCcomposites prepared by RMI" shows that the composites prepared by RMI melt infiltration process need to introduce an appropriate amount of matrix into the carbon fiber preform to protect the erosion of the fiber by the molten alloy during the melt infiltration process. The prepared composites have the characteristics of fast densification speed and high density, but the fiber structure will inevitably be damaged to a certain extent during the high-temperature reaction melt infiltration process.
[0044] It can be seen that the preparation method of ceramic-based composite materials in the related art cannot achieve the technical effects of short cycle, uniform component distribution, and complete fiber structure.
[0045] To this end, combined Figure 1 As shown, a method for preparing a continuous carbon fiber reinforced ultra-high temperature ceramic matrix composite material is provided, comprising:
[0046] Step 101: Mix a solvent, a dispersant and ceramic powder to prepare a ceramic slurry.
[0047] Step 102: Depositing an interface inside the fiber braided body to prepare a fiber preform.
[0048] Step 103: Inject the ceramic slurry in step 101 into the central area of the fiber preform in step 102, and then solidify and crack it to prepare a first intermediate.
[0049] Step 104: The ceramic slurry in step 101 is introduced into the edge area of the fiber preform in step 102 except the central area by vacuum impregnation and pressure impregnation, and then solidified and cracked to prepare a second intermediate.
[0050] Step 105: densification by using a precursor impregnation cracking process, introducing the precursor polymer solution into the second intermediate by impregnation, followed by curing and cracking, to convert the second intermediate into a silicon carbide ceramic component, thereby obtaining a densified continuous carbon fiber reinforced ultrahigh temperature ceramic matrix composite material.
[0051] Optionally, the solvent in step 101 is a first type solvent or a second type solvent, wherein the first type solvent includes one or more of deionized water, anhydrous ethanol, acetone, xylene, and toluene. The second type solvent includes one or more of polycarbosilane (PCS), polysilazane, polyborazane, and polysiloxane.
[0052] Optionally, the dispersant in step 101 includes one or more of trioctylphosphine oxide (TOPO), carboxymethyl cellulose (CMC), polyacrylamide (PAM), and polyvinyl alcohol (PVA).
[0053] Optionally, the ceramic powder in step 101 is boride, carbide or nitride. The content of ceramic powder in the ceramic slurry is 5-90wt%, the content of dispersant in the ceramic slurry is 0.5-10% of the mass of the ceramic powder, and the particle size of the ceramic powder is 0.05-50μm.
[0054] Optionally, the fiber preform in step 101 includes carbon fiber, 10iC fiber, silicon nitride fiber, glass fiber, oxide fiber or other ceramic fiber. The fiber preform is formed by two-dimensional lamination, three-dimensional needle-punched fiber or three-dimensional weaving, and the fiber content of the fiber preform is 10-75 vol%.
[0055] In the embodiments of the present application, Figure 2 As shown, C f Taking the composite material of UHTCs-SiC as an example, the preparation method of the composite material is described, including:
[0056] Step 201: depositing an interface on a needle-punched carbon fiber preform by chemical vapor infiltration, and controlling the interface thickness to be 50-600 nm.
[0057] Step 202: Prepare a PCS solution with a concentration of 0 to 70 wt%, add UHTC s powder with a particle size of 0.5 to 5 μm and CMC dispersant, mix well to obtain a ceramic slurry, and use a drum ball mill at a speed of 100 to 300 r / min for 12 to 24 hours to obtain the final ceramic slurry. -1 At a shear rate of , the viscosity is 100-1000mPa·s.
[0058] Step 203: Inject the ceramic slurry obtained in step 202 into the carbon fiber preform in step 201 in a dot matrix arrangement on a glue injection machine to obtain an injection embryo.
[0059] The injection spacing in the three mutually perpendicular X, Y and Z directions is 2-10 mm, the inner diameter of the needle is 0.2-1 mm, the injection time of the array point is 0.5-2.0 s, the injection pressure is 0.5-1.5 MPa, and the injection volume is 0.3-1.2 cm 3 .
[0060] Step 204: solidify the injected embryo obtained in step 203 at 100-400°C for 1-2 hours, and then pyrolyze at 600-1400°C for 1-4 hours at a heating rate of 2-5°C / min. The whole process is carried out in a fluid medium of Ar gas.
[0061] Step 205: C f / UHTCs-SiC composite intermediate, vacuum impregnation and pressure impregnation in the ceramic slurry obtained in step 202.
[0062] Among them, the vacuum degree of vacuum impregnation is controlled below -0.09Mpa, and the impregnation time is 0.5 to 1.5h; the pressure of pressure impregnation is controlled at 0.5 to 3MPa, and the impregnation time is 0.5 to 2h.
[0063] Step 206: Repeat the solidification and cracking process of step 204 to obtain a semi-densified C f / UHTCs-SiC composites.
[0064] Step 207: The semi-densified C obtained in step 206 f The / UHTCs-SiC composite material is vacuum impregnated and pressure impregnated in the PCS solution obtained in step 202, and the curing and cracking process in step 204 is repeated.
[0065] Among them, the vacuum degree of vacuum impregnation is controlled below -0.09Mpa, and the impregnation time is 0.5 to 1.5h; the pressure of pressure impregnation is controlled at 0.5 to 3MPa, and the impregnation time is 0.5 to 2h.
[0066] Step 208: Repeat the precursor impregnation and cracking process of step 207 5 to 8 times to obtain a densified C with an open porosity of 7 to 10%. f / UHTCs-SiC composites.
[0067] The present application provides a method for preparing a continuous carbon fiber reinforced ultra-high temperature ceramic matrix composite material C by combining slurry injection with precursor impregnation pyrolysis. f / UHTCs-SiC process method, after the fiber braid is deposited through the interface layer, the ceramic powder is introduced into the central area of the fiber preform by the injection process, and then the ceramic powder is introduced into the edge area of the fiber preform by slurry impregnation, so as to achieve uniform distribution of the ceramic matrix in the preform. Finally, the precursor impregnation and cracking process is adopted for densification. In this way, the present application has the advantages of short cycle, uniform distribution of components and complete fiber structure. In addition, the present application protects the structural integrity of the fiber during the preparation process, improves the uniform distribution of components inside the material, and can greatly shorten the preparation cycle of the composite material, meeting the needs of the industry.
[0068] Specifically, the beneficial effects of the present invention are embodied in the following aspects:
[0069] (1) The present invention provides a method for preparing C by combining slurry injection with precursor impregnation cracking. f The method for preparing UHTCs-SiC composite materials has the advantages of short preparation cycle, simple process, little fiber damage, low cost and high repeatability. It is a low-cost and short-cycle composite material preparation technology.
[0070] (2) C prepared by the method of the present invention f / UHTCs-SiC composites have high densification degree, uniform component distribution and high relative density.
[0071] (3) By adjusting the slurry ratio, regulating the slurry viscosity and the content and type of ceramic powder, combined with the process parameter adjustment, the ceramic content in the composite matrix can be regulated, thereby improving the performance of the fiber-reinforced ceramic matrix composite material. The flexural strength of the composite material is not less than 400 MPa and the fracture toughness is not less than 12 MPa·m 1 / 2 , under oxyacetylene ablation conditions of 2600-2700℃, the linear ablation rate is less than 1μm / s.
[0072] The above contents are specifically described below by the following examples and comparative examples:
[0073] Example 1
[0074] Step 1: Slurry preparation.
[0075] Take 60g of ZrB2 powder with a particle size of 1-3μm, add it to a beaker containing 40g of deionized water, add 0.5-10% of the mass of ZrB2 powder CMC dispersant, stir on a magnetic stirrer at 1200r / min for 30min, and then roller mill at 120r / min for 12h to obtain a uniformly mixed and stable ZrB2 ceramic slurry.
[0076] Step 2: The needle-punched carbon fiber preform is subjected to chemical vapor infiltration to deposit a pyrolytic carbon (PyC) interface. When the interface thickness reaches 500 nm, the deposition is stopped and heat treatment is performed.
[0077] Step 3: Use a dispensing machine to introduce the ZrB2 ceramic slurry obtained in step 1 into the carbon fiber preform after the deposition interface in step 2. The inner diameter of the needle is 0.9 mm, the distance between the injection points in the X and Y directions is 5 mm, the distance between the injection points in the Z direction is 5 mm, the injection time is 1 s, and the injection pressure is 0.5 MPa.
[0078] Step 4: Place the composite material obtained in step 3 in a drying oven and dry it at 80°C for 2 hours to prepare a composite material with a density of 2.5 g / cm 3 The porous C f / ZrB2 composite materials.
[0079] Step 5: Slurry Impregnation
[0080] The slurry impregnation treatment is divided into two steps: vacuum impregnation and pressure impregnation: first, the composite material in step 4 is placed in a glass drying dish, and the vacuum is evacuated to a pressure lower than -0.09MPa in the dish. After maintaining for 30 minutes, the porous composite material is immersed in the ZrB2 ceramic slurry in step 2 and maintained for 30 minutes. Then, the slurry and the composite material are placed in a closed container, pressurized to 3MPa, maintained for 0.5h, and then taken out, and the surface of the preform is wiped dry and dried.
[0081] Step 6: Repeat the drying process of step 4 to prepare a density of 2.7 g / cm 3 The porous C f / Zr B2 composite materials.
[0082] Step 7: Prepare a mixed solution with a mass ratio of SiC precursor to organic solvent of 1:1, where the organic solvent is xylene.
[0083] Step 8: Precursor impregnation pyrolysis method to generate SiC densification: First, the porous composite material in step 6 is placed in a glass drying dish, and the pressure in the dish is evacuated to less than -0.09MPa. After maintaining for 30min, the porous composite material is immersed in the PCS solution in step 7 and maintained for 30min. Then, the PCS solution and the composite material are placed in a sealed container, pressurized to 0.5MPa, maintained for 0.5h, and then taken out, and the surface is wiped dry and dried.
[0084] Step 9: solidify the impregnated embryo obtained in step 8 at 400°C, keep warm for 1-2 hours, and then crack at 1400°C, keep warm for 1-4 hours, with a heating rate of 2-5°C / min, and the whole process is carried out in a fluid medium of Ar gas.
[0085] Step 10: Repeat the precursor impregnation and cracking process of step 8 and step 9 for 5 times to obtain an open porosity of 10% and a density of 3.1 g / cm 3 C f / ZrB2-SiC composite materials.
[0086] Comparative Example 1
[0087] Step 1: Prepare a 1.4 g / cm2 film using the CVI process 3 The porous C / SiC composite preform has a pyrolytic carbon interface layer thickness of 150nm-250nm, an open porosity of about 40%, a carbon fiber volume fraction of about 30%, and is ultrasonically cleaned for 1 hour using alcohol as a cleaning agent and dried at 150°C for 1 hour.
[0088] Step 2: Use 50 mL of xylene, 4 mL of liquid PCS, 30 g of ZrB2 powder, and dispersant BYK-057, which is 3% of the powder mass fraction and 0.95 g in mass. Ultrasonic disperse the slurry for 1 h, and mill it for 12 h at a planetary ball mill speed of 250 r / min.
[0089] Step 3: The slurry was vacuum impregnated into the porous C / SiC composite preform for 0.5 h at a vacuum degree of -0.09 MPa, and then the vacuum impregnated composite was impregnated for another 1 h at a pressure of 0.8 MPa, and then dried at 150 °C for 1 h.
[0090] Step 4: Repeat step 3 until the weight gain of the sample does not exceed 3%.
[0091] Step 5: prepare a mixed solution with a mass ratio of SiC precursor to organic solvent of 1:1, wherein the organic solvent is xylene, and use the mixed solution to vacuum pressure impregnate the composite material obtained in step 4. The vacuum pressure impregnation is the same as step 3, and the pyrolysis process is a heating rate of 5°C / min, a pyrolysis temperature of 1400°C, and a pyrolysis time of 2h.
[0092] Step 6: Repeat step 5 three times to achieve final densification.
[0093] Comparative Example 1 prepared C f The apparent density of ZrB2-SiC composite material can reach 2.40g / cm 3 The open porosity is less than 13%, and the volume fraction of ZrB2 matrix in the composite material is about 15%. The bending strength is 230-400MPa, and the fracture toughness is 1.39-8.20MPa·m 1 / 2 According to the GJB323B-2018 ablation material ablation test method test standard, at a heat flux density of 4.18MW / m 2 After 20s of oxyacetylene ablation test, the mass ablation rate was 3.5mg / s and the line ablation rate was about 3.1μm / s.
[0094] Compared with Comparative Example 1, Example 1 prepared C f The cycle of the / ZrB2-SiC composite material is only 140h, the content of ultra-high temperature powder is 30vol%, the relative density reaches 91.5%, the bending strength is increased by 10%, the fracture toughness is increased by 30%, and the ablation resistance is increased by 80%. At a heat flux of 4.18MW / m 2 After 20s of oxyacetylene ablation test, the mass ablation rate of the composite material was less than 2mg / s; the line ablation rate was less than 1μm / s. Figure 3 The porous C prepared by slurry injection in Example 1 f CT images of / ZrB2-SiC composite materials: (a) 3D reconstructed model; (b) XY plane ray diagram; it can be seen that the components are evenly distributed. Figure 4 Example 1C f / ZrB2-SiC composite material microstructure: (a) web layer area; (b) fiber bundle area; it can be seen that the components are evenly distributed and the fiber structure is complete. Figure 5 The three-dimensional morphology of the ablated surface of the Cf / ZrB2-SiC composite material in Example 1 is shown in FIG. f / ZrB2-SiC composite materials have excellent anti-ablation performance.
[0095] It is shown that the present invention protects the structural integrity of the fiber during the preparation process, improves the mechanical properties of the material, improves the uniform distribution of components inside the material, enhances the anti-ablation ability of the composite material, and greatly shortens the preparation cycle of the composite material, which can meet the needs of the industry.
[0096] Example 2
[0097] Step 1: Slurry preparation.
[0098] Prepare a PCS solution with a mass ratio of SiC precursor to xylene of 1:1, take 60g of ZrB2 powder with a particle size of 1-3μm, add it into a beaker containing 40g of PCS solution, add 0.5-10% of the mass of ZrB2 powder CMC dispersant, stir for 30min on a magnetic stirrer at 1200r / min, and then roller mill for 12h at a speed of 120r / min to obtain a uniformly mixed and stable ZrB2 ceramic slurry.
[0099] Step 2: The needle-punched carbon fiber preform is subjected to chemical vapor infiltration to deposit a pyrolytic carbon (PyC) interface. When the interface thickness reaches 500 nm, the deposition is stopped and heat treatment is performed.
[0100] Step 3: Use a dispensing machine to introduce the ZrB2 ceramic slurry obtained in step 1 into the carbon fiber preform after the deposition interface in step 2. The inner diameter of the needle is 0.9 mm, the distance between the injection points in the X and Y directions is 5 mm, the distance between the injection points in the Z direction is 5 mm, the injection time is 1 s, and the injection pressure is 0.5 MPa.
[0101] Step 4: The injected embryo obtained in step 3 was solidified at 100-400°C for 1-2 hours, and then cracked at 600-1400°C for 1-4 hours at a heating rate of 2-5°C / min. The whole process was carried out in an Ar gas fluid medium to prepare a 2.4 g / cm 3 The porous C f / ZrB2-SiC composite materials.
[0102] Step 5: Slurry Impregnation
[0103] The slurry impregnation treatment is divided into two steps: vacuum impregnation and pressure impregnation: first, the composite material in step 4 is placed in a glass drying dish, and the vacuum is evacuated to a pressure lower than -0.09MPa in the dish. After maintaining for 30 minutes, the porous composite material is immersed in the ZrB2 ceramic slurry in step 2 and maintained for 30 minutes. Then, the slurry and the composite material are placed in a closed container, pressurized to 3MPa, maintained for 0.5h, and then taken out, and the surface of the preform is wiped dry and dried.
[0104] Step 6: Repeat the curing and cracking process in step 4 to prepare a product with a density of 2.7 g / cm 3 The porous C f / ZrB2-SiC composite materials.
[0105] Step 7: Precursor impregnation pyrolysis method to generate SiC densification: First, the porous composite material in step 6 is placed in a glass drying dish, and the pressure in the dish is evacuated to less than -0.09 MPa. After maintaining for 30 min, the porous composite material is immersed in the PCS solution in step 1 and maintained for 30 min. Then, the PCS solution and the composite material are placed in a sealed container, pressurized to 0.8 MPa, maintained for 0.5 h, and then taken out.
[0106] Step 9: solidify the impregnated embryo obtained in step 8 at 400°C, keep warm for 1-2 hours, and then crack at 1400°C, keep warm for 1-4 hours, with a heating rate of 2-5°C / min, and the whole process is carried out in a fluid medium of Ar gas.
[0107] Step 10: Repeat the precursor impregnation and cracking process of step 8 and step 9 for 7 times to obtain an open porosity of 9% and a density of 2.9 g / cm 3 C f / ZrB2-SiC composite materials.
[0108] Compared with the SI process, the C f During the preparation process of the ZrB2-SiC composite material, the problem of uneven distribution of components inside the embryo caused by the introduction of high solid content slurry was avoided, and the ablation resistance of the composite material was effectively improved.
[0109] Example 3
[0110] Step 1: Slurry preparation.
[0111] Prepare a PCS solution with a SiC precursor and xylene ratio of 1:1, prepare a mixed ceramic powder with a ZrB2 and HfB2 ratio of 1:1, take 60g of the mixed ceramic powder, add it into a beaker containing 40g of PCS solution, add 0.5-10% of the powder mass of CMC dispersant, stir on a magnetic stirrer at 1200r / min for 30min, and then drum ball mill at 120r / min for 12h to obtain a uniformly mixed and stable ceramic slurry.
[0112] Step 2: The needle-punched carbon fiber preform is subjected to chemical vapor infiltration to deposit a pyrolytic carbon (PyC) interface. When the interface thickness reaches 500 nm, the deposition is stopped and heat treatment is performed.
[0113] Step 3: Use a dispensing machine to introduce the ZrB2 ceramic slurry obtained in step 1 into the carbon fiber preform after the deposition interface in step 2. The inner diameter of the needle is 0.9 mm, the distance between the injection points in the X and Y directions is 5 mm, the distance between the injection points in the Z direction is 5 mm, the injection time is 1 s, and the injection pressure is 0.5 MPa.
[0114] Step 4: The injected embryo obtained in step 3 was solidified at 100-400°C for 1-2 hours, and then cracked at 600-1400°C for 1-4 hours at a heating rate of 2-5°C / min. The whole process was carried out in an Ar gas fluid medium to prepare a 2.6 g / cm 3 The porous C f / ZrB2-HfB2-SiC composite materials.
[0115] Step 5: Slurry Impregnation
[0116] The slurry impregnation treatment is divided into two steps: vacuum impregnation and pressure impregnation: first, the composite material in step 4 is placed in a glass drying dish, and the vacuum is evacuated to a pressure lower than -0.09 MPa in the dish. After maintaining for 30 minutes, the porous composite material is immersed in the ceramic slurry in step 2 and maintained for 30 minutes. Then, the slurry and the composite material are placed in a sealed container, pressurized to 3 MPa, maintained for 0.5 hours, and then taken out, and the surface of the preform is wiped dry and dried.
[0117] Step 6: Repeat the curing and cracking process in step 4 to prepare a product with a density of 2.9 g / cm 3 The porous C f / ZrB2-HfB2-SiC composite materials.
[0118] Step 7: Precursor impregnation pyrolysis method to generate SiC densification: First, the porous composite material in step 6 is placed in a glass drying dish, and the pressure in the dish is evacuated to less than -0.09 MPa. After maintaining for 30 min, the porous composite material is immersed in the PCS solution in step 1 and maintained for 30 min. Then, the PCS solution and the composite material are placed in a sealed container, pressurized to 0.8 MPa, maintained for 0.5 h, and then taken out.
[0119] Step 9: solidify the impregnated embryo obtained in step 8 at 400°C, keep warm for 1-2 hours, and then crack at 1400°C, keep warm for 1-4 hours, with a heating rate of 2-5°C / min, and the whole process is carried out in a fluid medium of Ar gas.
[0120] Step 10: Repeat the precursor impregnation and cracking process of step 8 and step 9 for 7 times to obtain an open porosity of 10% and a density of 3.1 g / cm 3 C f / ZrB2-HfB2-SiC composite materials.
[0121] Compared with Comparative Example 1, the present embodiment prepares C f The content of ultra-high temperature powder of the / ZrB2-HfB2-SiC composite material is 30vol.%, and the ablation resistance is improved by 140%.
[0122] Example 4
[0123] Step 1: Slurry preparation.
[0124] Prepare a PCS solution with a SiC precursor and xylene ratio of 1:1, prepare a mixed ceramic powder with a ZrB2 and HfB2 ratio of 1:1, take 80g of the mixed ceramic powder, add it into a beaker containing 20g of PCS solution, add 0.5-10% of the powder mass of CMC dispersant, stir on a magnetic stirrer at 1200r / min for 30min, and then drum ball mill at 120r / min for 12h to obtain a uniformly mixed and stable ceramic slurry.
[0125] Step 2: The needle-punched carbon fiber preform is subjected to chemical vapor infiltration to deposit a pyrolytic carbon (PyC) interface. When the interface thickness reaches 500 nm, the deposition is stopped and heat treatment is performed.
[0126] Step 3: Use a dispensing machine to introduce the ZrB2 ceramic slurry obtained in step 1 into the carbon fiber preform after the deposition interface in step 2. The inner diameter of the needle is 0.9 mm, the distance between the injection points in the X and Y directions is 5 mm, the distance between the injection points in the Z direction is 5 mm, the injection time is 1 s, and the injection pressure is 0.5 MPa.
[0127] Step 4: The injected embryo obtained in step 3 was solidified at 100-400°C for 1-2 hours, and then cracked at 600-1400°C for 1-4 hours at a heating rate of 2-5°C / min. The whole process was carried out in an Ar gas fluid medium to prepare a 2.7 g / cm 3 The porous C f / ZrB2-HfB2-SiC composite materials.
[0128] Step 5: Slurry Impregnation
[0129] The slurry impregnation treatment is divided into two steps: vacuum impregnation and pressure impregnation: first, the composite material in step 4 is placed in a glass drying dish, and the vacuum is evacuated to a pressure lower than -0.09 MPa in the dish. After maintaining for 30 minutes, the porous composite material is immersed in the ceramic slurry in step 2 and maintained for 30 minutes. Then, the slurry and the composite material are placed in a sealed container, pressurized to 3 MPa, maintained for 0.5 hours, and then taken out, and the surface of the preform is wiped dry and dried.
[0130] Step 6: Repeat the solidification and cracking process in step 4 to prepare a density of 3.1 g / cm 3 The porous C f / ZrB2-HfB2-SiC composite materials.
[0131] Step 7: Precursor impregnation pyrolysis method to generate SiC densification: First, the porous composite material in step 6 is placed in a glass drying dish, and the pressure in the dish is evacuated to less than -0.09 MPa. After maintaining for 30 min, the porous composite material is immersed in the PCS solution in step 1 and maintained for 30 min. Then, the PCS solution and the composite material are placed in a sealed container, pressurized to 0.8 MPa, maintained for 0.5 h, and then taken out.
[0132] Step 9: solidify the impregnated embryo obtained in step 8 at 400°C, keep warm for 1-2 hours, and then crack at 1400°C, keep warm for 1-4 hours, with a heating rate of 2-5°C / min, and the whole process is carried out in a fluid medium of Ar gas.
[0133] Step 10: Repeat the precursor impregnation and cracking process of step 8 and step 9 for 7 times to obtain an open porosity of 9.5% and a density of 3.3 g / cm 3 C f / ZrB2-HfB2-SiC composite materials.
[0134] This example is compared with Example 3 to prepare C f The ultra-high temperature ceramic component content of the / ZrB2-HfB2-SiC composite material is increased by 16.2%, and its ablation resistance is improved by 40%.
[0135] Comparative Example 2
[0136] Step 1: Slurry preparation.
[0137] Take 60g of ZrB2 powder with a particle size of 1-3μm, add it to a beaker containing 40g of deionized water, add 0.5-10% of the mass of ZrB2 powder CMC dispersant, stir on a magnetic stirrer at 1200r / min for 30min, and then roller mill at 120r / min for 12h to obtain a uniformly mixed and stable ZrB2 ceramic slurry.
[0138] Step 2: The needle-punched carbon fiber preform is subjected to chemical vapor infiltration to deposit a pyrolytic carbon (PyC) interface. When the interface thickness reaches 500 nm, the deposition is stopped and heat treatment is performed.
[0139] Step 3: Use a dispensing machine to introduce the ZrB2 ceramic slurry obtained in step 1 into the carbon fiber preform after the deposition interface in step 2. The inner diameter of the needle is 1.45 mm, the distance between the injection points in the X and Y directions is 5 mm, the distance between the injection points in the Z direction is 5 mm, the injection time is 1 s, and the injection pressure is 1 MPa.
[0140] Step 4: Place the composite material obtained in step 3 in a drying oven and dry it at 80°C for 2 hours to prepare a composite material with a density of 2.6 g / cm 3 The porous Cf / ZrB2 composite materials.
[0141] Step 5: Slurry Impregnation
[0142] The slurry impregnation treatment is divided into two steps: vacuum impregnation and pressure impregnation: first, the composite material in step 4 is placed in a glass drying dish, and the vacuum is evacuated to a pressure lower than -0.09MPa in the dish. After maintaining for 30 minutes, the porous composite material is immersed in the ZrB2 ceramic slurry in step 2 and maintained for 30 minutes. Then, the slurry and the composite material are placed in a closed container, pressurized to 3MPa, maintained for 0.5h, and then taken out, and the surface of the preform is wiped dry and dried.
[0143] Step 6: Repeat the drying process of step 4 to prepare a density of 2.8g / cm 3 The porous C f / Zr B2 composite materials.
[0144] Step 7: Prepare a mixed solution with a mass ratio of SiC precursor to organic solvent of 1:1, where the organic solvent is xylene.
[0145] Step 8: Precursor impregnation pyrolysis method to generate SiC densification: First, the porous composite material in step 6 is placed in a glass drying dish, and the pressure in the dish is evacuated to less than -0.09MPa. After maintaining for 30min, the porous composite material is immersed in the PCS solution in step 7 and maintained for 30min. Then, the PCS solution and the composite material are placed in a sealed container, pressurized to 0.5MPa, maintained for 0.5h, and then taken out, and the surface is wiped dry and dried.
[0146] Step 9: solidify the impregnated embryo obtained in step 8 at 400°C, keep warm for 1-2 hours, and then crack at 1400°C, keep warm for 1-4 hours, with a heating rate of 2-5°C / min, and the whole process is carried out in a fluid medium of Ar gas.
[0147] Step 10: Repeat the precursor impregnation and cracking process of step 8 and step 9 for 5 times to obtain an open porosity of 11% and a density of 3.0 g / cm 3 C f / ZrB2-SiC composite materials.
[0148] Comparative Example 2 Compared with Example 1, the C f The volume density and open porosity of the intermediate of / SiC-ZrB2 composite material are similar, but because the needle diameter exceeds 1mm, f Obvious holes are left on the surface of the / ZrB2-SiC composite material, which greatly affects the bending strength and ablation resistance of the material.
[0149] In summary, the present application provides a new carbon fiber reinforced ultra-high temperature ceramic matrix composite material process, which combines slurry injection and slurry impregnation processes to achieve rapid and uniform introduction of ceramic components during material preparation, and then densification is achieved through precursor impregnation cracking to obtain a carbon fiber reinforced ceramic matrix composite material. This application can obtain a well-densified carbon fiber reinforced ceramic matrix composite material, which can solve the problems of long preparation cycle, high cost and poor densification effect existing in the current precursor impregnation cracking, and lay an industrial foundation for the rapid preparation of composite materials.
[0150] The disclosed embodiment provides a continuous carbon fiber reinforced ultra-high temperature ceramic-based composite material prepared by the preparation method of the present application.
[0151] The above description and the accompanying drawings fully illustrate the embodiments of the present disclosure so that those skilled in the art can practice them. Other embodiments may include structural, logical, electrical, process and other changes. The embodiments represent only possible changes. Unless explicitly required, separate components and functions are optional, and the order of operation may vary. The parts and features of some embodiments may be included in or replace the parts and features of other embodiments. Moreover, the words used in this application are only used to describe the embodiments and are not used to limit the claims. As used in the description of the embodiments and the claims, unless the context clearly indicates, the singular forms of "a", "an" and "the" are intended to include plural forms as well. Similarly, the term "and / or" as used in this application refers to any and all possible combinations of listings containing one or more associated ones. In addition, when used in the present application, the term "comprise" and its variants "comprises" and / or comprising refer to the presence of stated features, wholes, steps, operations, elements, and / or components, but do not exclude the presence or addition of one or more other features, wholes, steps, operations, elements, components and / or groups thereof. In the absence of further restrictions, the elements defined by the sentence "comprising a ..." do not exclude the presence of other identical elements in the process, method or device comprising the elements. In this article, each embodiment may focus on the differences from other embodiments, and the same and similar parts between the various embodiments may refer to each other. For the methods, products, etc. disclosed in the embodiments, if they correspond to the method part disclosed in the embodiments, then the relevant parts can refer to the description of the method part.
[0152] Those skilled in the art will appreciate that the units and algorithm steps of each example described in conjunction with the embodiments disclosed herein can be implemented in electronic hardware, or a combination of computer software and electronic hardware. Whether these functions are performed in hardware or software may depend on the specific application and design constraints of the technical solution. The technicians may use different methods for each specific application to implement the described functions, but such implementations should not be considered to exceed the scope of the embodiments of the present disclosure. The technicians may clearly understand that, for the convenience and simplicity of description, the specific working processes of the systems, devices and units described above may refer to the corresponding processes in the aforementioned method embodiments, and will not be repeated here.
[0153] In the embodiments disclosed herein, the disclosed methods and products (including but not limited to devices, equipment, etc.) can be implemented in other ways. For example, the device embodiments described above are only schematic. For example, the division of the units can be only a logical function division. There may be other division methods in actual implementation, such as multiple units or components can be combined or integrated into another system, or some features can be ignored or not executed. In addition, the coupling or direct coupling or communication connection between each other shown or discussed can be through some interfaces, indirect coupling or communication connection of devices or units, which can be electrical, mechanical or other forms. The units described as separate components may or may not be physically separated, and the components displayed as units may or may not be physical units, that is, they may be located in one place, or they may be distributed on multiple network units. Some or all of the units may be selected according to actual needs to implement this embodiment. In addition, each functional unit in the embodiment of the present disclosure may be integrated in a processing unit, or each unit may exist physically alone, or two or more units may be integrated in one unit.
[0154] The flowchart and block diagram in the accompanying drawings show the possible architecture, function and operation of the system, method and computer program product according to the embodiment of the present disclosure. In this regard, each box in the flowchart or block diagram can represent a module, a program segment or a part of the code, and the module, the program segment or a part of the code contains one or more executable instructions for realizing the specified logical function. In some alternative implementations, the functions marked in the box can also occur in a different order from the order marked in the accompanying drawings. For example, two consecutive boxes can actually be executed substantially in parallel, and they can sometimes be executed in the opposite order, which can depend on the functions involved. In the description corresponding to the flowchart and the block diagram in the accompanying drawings, the operations or steps corresponding to different boxes can also occur in a different order from the order disclosed in the description, and sometimes there is no specific order between different operations or steps. For example, two consecutive operations or steps can actually be executed substantially in parallel, and they can sometimes be executed in the opposite order, which can depend on the functions involved. Each block in the block diagrams and / or flowcharts, and combinations of blocks in the block diagrams and / or flowcharts, may be implemented by a dedicated hardware-based system that performs the specified functions or actions, or may be implemented by a combination of dedicated hardware and computer instructions.
Claims
1. A method for preparing a continuous carbon fiber reinforced ultra-high temperature ceramic matrix composite material, characterized in that: include: S1: mixing a solvent, a dispersant and a ceramic powder to prepare a ceramic slurry; S2: depositing an interface inside the fiber braid to prepare a fiber preform; S3: Injecting the ceramic slurry in step S1 into the central area of the fiber preform in step S2, followed by curing and cracking to prepare a first intermediate; S4: introducing the ceramic slurry in step S1 into the edge area of the fiber preform in step S2 except the central area by vacuum impregnation and pressure impregnation, and then curing and cracking to prepare a second intermediate; S5: Densification is carried out by using a precursor impregnation and cracking process. The precursor polymer solution is introduced into the second intermediate by impregnation, and then cured and cracked to convert the second intermediate into a silicon carbide ceramic component to obtain a densified continuous carbon fiber reinforced ultra-high temperature ceramic matrix composite material.
2. The preparation method according to claim 1, characterized in that: In step S1, the solvent is a first type solvent or a second type solvent, the first type solvent includes one or more of deionized water, anhydrous ethanol, acetone, xylene, and toluene; the second type solvent includes one or more of polycarbosilane (PCS), polysilazane, polyborazane, and polysiloxane; The dispersant includes one or more of trioctylphosphine oxide (TOPO), carboxymethyl cellulose (CMC), polyacrylamide (PAM), and polyvinyl alcohol (PVA).
3. The preparation method according to claim 1, characterized in that: In step S1, the ceramic powder is a boride, a carbide or a nitride; The content of ceramic powder in the ceramic slurry is 5 to 90 wt %; The content of the dispersant in the ceramic slurry is 0.5-10% of the mass of the ceramic powder; The particle size of the ceramic powder is 0.05-50 μm.
4. The preparation method according to claim 1, characterized in that: In step S1, the fiber preform includes carbon fiber, SiC fiber, silicon nitride fiber, glass fiber or oxide fiber; The fiber preform is formed by two-dimensional lamination, three-dimensional needle-punched fiber or three-dimensional weaving; The fiber content of the fiber preform is 10-75 vol%.
5. The preparation method according to claim 1, characterized in that: In step S2, the material of the interface includes one or more of pyrolytic carbon PyC, boron nitride BN, silicon carbide SiC, and silicon nitride Si3N4; The deposition thickness of the interface is 50-600 nm.
6. The preparation method according to claim 1, characterized in that: In step S3, the ceramic slurry is arranged in a dot matrix in the central area of the fiber preform, and the injection dot matrix includes a circular arrangement, a rectangular arrangement or an irregular arrangement; In step S3, the curing and cracking processes are both carried out in an inert gas, wherein the curing temperature is 80-400° C., and the holding time is 0.5-3 h; the cracking temperature is 600-1400° C., and the holding time is 0.5-3 h.
7. The preparation method according to claim 6, characterized in that: In step S3, during injection, the injection spacing along three mutually perpendicular directions is 2-10 mm, the inner diameter of the needle used for injection is 0.2-1 mm, the injection time of the injection array is 0.5-2.0 s, and the injection pressure is 0.5-1.5 MPa.
8. The preparation method according to claim 1, characterized in that: In step S4, the vacuum impregnation and pressure impregnation include: First, the first intermediate is placed in an environment with a vacuum degree lower than -0.09 MPa and allowed to stand, and then placed in the ceramic slurry in step S1 for pressure impregnation, wherein the pressure of the pressure impregnation is 0.5 to 3 MPa, and the time of the pressure impregnation is 0.5 to 2 hours; In step S4, the curing and cracking process is carried out in an inert gas, wherein the curing temperature is 80-400°C, the holding time is 0.5-3h, and the cracking temperature is 600-1400°C, the holding time is 0.5-3h.
9. The preparation method according to claim 1, characterized in that: In step S5, the precursor polymer includes one or more of polycarbosilane, polysilazane, polyborazane, and polysiloxane; In step S5, the impregnation includes vacuum impregnation and pressure impregnation, and the vacuum impregnation and pressure impregnation include: Firstly, the first intermediate is placed in an environment with a vacuum degree lower than -0.09 MPa and allowed to stand, and then placed in a precursor polymer solution for pressure impregnation, wherein the pressure of the pressure impregnation is 0.5 to 3 MPa and the time of the pressure impregnation is 0.5 to 2 hours; In step S5, the curing and cracking processes are both carried out in an inert gas, wherein the curing temperature is 80-400° C., the holding time is 0.5-4 h, and the cracking temperature is 600-1400° C., the holding time is 0.5-3 h.
10. A continuous carbon fiber reinforced ultrahigh temperature ceramic matrix composite material prepared by the preparation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Preparation method for fiber-reinforced superhigh temperature ceramic matrix composite
CN103964882A
Ultra-high-temperature ceramic-based composite material with high thermal conductivity, strong bonding force and ablation resistance and preparation method thereof
CN111454073A
High-entropy ceramic-based composite material and preparation method thereof
CN117567158A
Continuous fiber reinforced ceramic matrix composite material and preparation method thereof
CN117567165A
Method for manufacturing high-density fiber reinforced ceramic composite materials
EP2543650A1
Cited By
Fiber-reinforced ultrahigh-temperature ceramic-based composite material and preparation method thereof
CN119751103A
A fiber-reinforced ultra-high temperature ceramic-based composite material and its preparation method
CN119751103B
Integrated preparation method of fiber-reinforced ultrahigh-temperature ceramic composite material
CN120535315A