High-temperature and high-pressure synthesis method of carbon fiber reinforced and toughened ceramic composite material

By coating the amorphous silicon oxide film of nano-silica powder on the surface of nickel-plated carbon fiber and adopting high-temperature and high-pressure technology, the problem of insufficient brittleness and interface bonding ability of ceramic materials is solved, and the strength and toughness and temperature resistance of ceramic composite materials are significantly improved. Uniform nanograin structure.

CN118908742AActive Publication Date: 2024-11-08JILIN UNIVERSITY

Patent Information

Application Number
CN202411018610.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-08
Estimated Expiration
2044-07-29

AI Technical Summary

Technical Problem

Traditional ceramic materials have high brittleness and low toughness at high temperatures, and poor carbon fiber surfactivity leads to insufficient interfacial bonding ability with the ceramic matrix, making it difficult to fully exert the enhanced toughening effect.

Method used

The sol-gel method is used to coat the nickel-plated carbon fiber surface with amorphous silicon oxide film, and is prepared by high-temperature and high-pressure technology to regulate the thickness and structure of the gel layer, and improve the bonding strength of carbon fiber and ceramic matrix and the compactness of the material. sex.

Benefits of technology

It significantly improves the strength, temperature resistance and interface bonding strength of ceramic composite materials, reduces the sintering temperature and preparation time, forms uniform nanograin structure, and enhances the overall performance of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908742A_ABST
    Figure CN118908742A_ABST
Patent Text Reader

Abstract

The invention discloses a high-temperature and high-pressure preparation method of a carbon fiber reinforced and toughened ceramic composite material, and belongs to the technical field of preparation of ceramic composite materials. The method comprises the following steps: firstly, carrying out surface coating treatment on nickel-plated carbon fibers: adding a silane coupling agent into an alcohol-water solution, fully hydrolyzing, then adding nickel-plated PAN-based carbon fibers and nano silicon powder, carrying out suction filtration on the solution after the reaction is completed, drying to obtain modified carbon fibers with a surface film layer structure of Ni-Si-SiO2, loading the modified carbon fibers into an assembly block of a cubic press, and carrying out vacuum drying to obtain the nickel-plated PAN-based carbon fibers with the surface film layer structure of Ni-Si-SiO2. And putting the mixture into a cubic press, and sintering and pressing for 10-30 minutes under the conditions that the temperature is 1100-1500 DEG C and the pressure is 1-5 GPa to obtain the block reinforced and toughened ceramic composite material. The phase structure and the coating thickness of the gel layer on the surface of the carbon fiber are adjusted by adding the nano silicon powder, the brittleness of the ceramic phase material is improved, and the silicon oxide-based ceramic composite material with the overall organization structure being nanocrystal grains and having the self-lubricating / anti-attrition, heat-resistant and corrosion-resistant functions is synthesized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of preparation of ceramic composite materials, and relates to a reinforced / toughened / self-lubricating ceramic composite material prepared by high temperature and high pressure (HTHP) technology, using nickel-plated polyacrylonitrile-based (PAN) carbon fiber with surface metal-non-metallization composite modification as a toughening and reinforcing phase, in-situ generated silicon oxide as a ceramic matrix phase, and nano silicon powder as a coating increment and reaction adjustment phase. Background Art

[0002] Ceramic materials refer to a class of inorganic non-metallic materials made by forming and high-temperature sintering of natural or synthetic compounds. They have excellent properties such as high melting point, high hardness, high wear resistance and oxidation resistance. There are many types of ceramic materials, which are widely used in machinery, chemical industry, aerospace and other fields. With the continuous expansion of application scenarios, higher requirements are put forward for the strength, toughness, temperature resistance and wear resistance of ceramic materials. Ceramic materials prepared by traditional raw materials and high temperature-normal pressure processes are difficult to overcome the shortcomings of coarse grains, large brittleness and low toughness. To this end, people have carried out a series of attempts to strengthen and toughen ceramic materials. For example, by optimizing technical processes and designing fine microstructures to reduce the number of pores / cracks in ceramics to improve the brittleness of materials; by refining grains to improve the toughness of materials; at the same time, adding an appropriate amount of functional additives to the matrix material to promote densification, inhibit abnormal grain growth, and improve the strength and toughness of materials; and adding suitable reinforcing / toughening phases to the ceramic matrix to improve the strength and toughness of materials. Among the commonly used toughening materials, carbon fiber is a filamentary carbon material with a carbon content of more than 90%. It has the characteristics of light weight, high specific elasticity, high specific strength, high temperature resistance, friction resistance and corrosion resistance. Therefore, it is often selected as a reinforcing material for compounding with resin, metal or ceramic to improve the comprehensive mechanical properties of the material. However, carbon fiber has poor surface activity and does not wet with the heterogeneous ceramic matrix. The bonding ability between the heterogeneous phase interfaces of composite materials is a key factor restricting the performance of the material. Therefore, how to improve the surface activity of carbon fiber and improve its interfacial bonding ability with heterogeneous materials is a key factor in giving full play to the reinforcement / toughening performance of carbon fiber. In this regard, the carbon fiber raw material needs to be surface modified before compounding to increase the number of surface active sites of carbon fiber, which can effectively improve its interfacial wettability and bonding ability with heterogeneous materials.

[0003] Patent CN 113185313 B provides a carbon fiber reinforced ceramic matrix composite material and a preparation method thereof, wherein a carbon fiber preform is impregnated with boron carbide colloid, and after aging treatment, it is immersed again in a prefabricated reaction solution including silicon carbide and an ultra-high temperature ceramic precursor. The carbon fiber blank obtained after the curing treatment is heat-treated, and the obtained carbon fiber reinforced ceramic matrix composite material has the advantages of ultra-high temperature resistance, high overall strength and good fracture toughness. However, after the precursor is pyrolyzed at high temperature, a particle stacking structure is formed on the fiber surface, and the bonding force with the fiber is poor; the problem of large ceramic phase particle size and high porosity between particles after the pyrolysis of the ultra-high temperature ceramic precursor cannot be completely avoided, and it is more obvious after the composite material is ablated at high temperature. Patent CN117326880 A provides a high temperature and high pressure preparation method for a nickel-plated carbon fiber / silicon oxide composite material, after the nickel-plated carbon fiber is surface-modified with a silane coupling agent, a high temperature and high pressure synthesis technology is used to obtain a carbon fiber reinforced silicon oxide ceramic composite material with high strength and toughness. However, the gel film layer coated on the surface of nickel-plated carbon fiber by the condensation reaction of tetraethyl orthosilicate is thin, and a large number of residual active oxygen groups reduce the phase conversion rate of the coating layer during high temperature and high pressure, and oxidize and destroy the nickel-plated layer, thereby reducing the strength of the composite material. Therefore, it is also necessary to solve the problem of effectively thickening the gel coating layer in order to further adjust the amount, structure and properties of the ceramic matrix phase.

[0004] In the process of coating amorphous nano silicon oxide film on the surface of nickel-plated carbon fiber by sol-gel method with silane coupling agent as reaction precursor, nano silicon powder is added to the precursor solution, thereby increasing the coating thickness, consuming free oxygen in the silane film, and increasing the ratio of carbon fiber to ceramic matrix, thereby regulating the structure and physical properties of the composite material. In particular, the present invention adopts high temperature and high pressure (HTHP) technology for synthesis and preparation, and the addition of nano silicon powder can increase the number of in-situ nucleation cores of silicon oxide, greatly reduce the synthesis temperature, and inhibit the coarsening growth of grains under the action of high temperature and high pressure, so as to achieve the regulation effect of increasing the in-situ generation reaction ratio and refining the matrix structure, improve the density and toughness of ceramic composite materials, solve the application technology problem of carbon fiber reinforcement / toughening, and on this basis, can further prepare new superhard material products such as high temperature resistant abrasive tools with superhard abrasive grains such as diamond / boron nitride as hard phase. Summary of the invention

[0005] In order to solve the shortcomings of the prior art, adjust the physical structure and coating thickness of the gel layer on the surface of the carbon fiber, refine the gel layer organization, enhance the reaction activity of the gel layer, improve the brittleness of the ceramic matrix phase, and improve the bonding strength and overall toughness / temperature resistance of the heterogeneous phase interface of the ceramic composite material. The present invention provides a high temperature and high pressure preparation method for carbon fiber reinforced toughened ceramic composite material. First, the carbon fiber is surface coated with carbon-philic element nickel (Ni), and a carbon-philic active metal layer is established on the surface of the carbon fiber. Then, a layer of amorphous silica gel film containing elemental nano silicon powder is coated on the surface of the nickel-plated carbon fiber by a sol-gel method, and the thickness of the amorphous film layer is regulated by combining the amount and distribution state of the nano silicon powder. Then, a high temperature and high pressure (HTHP) synthesis method is used to place it in a six-sided top press to sinter a composite sheet sample with a size of φ10×1mm, and a carbon fiber reinforced toughened, self-lubricating / friction-reducing, heat-resistant / corrosion-resistant silica-based ceramic composite material is prepared. The size of the sintered product prepared by this method can be adjusted according to the needs of the actual workpiece.

[0006] The specific technical solutions of the present invention are as follows:

[0007] A high-temperature and high-pressure preparation method for a carbon fiber reinforced toughened ceramic composite material, comprising the following specific steps: adding a silane coupling agent to an alcohol aqueous solution, stirring continuously for 2 to 12 hours at 40 to 100° C., adding nickel-plated PAN-based carbon fiber and nano silicon powder after sufficient hydrolysis, stirring continuously for 2 to 12 hours at 40 to 100° C., filtering and drying the solution after the reaction is completed to obtain nano amorphous silicon oxide coated modified carbon fiber, installing the obtained modified carbon fiber in an assembly block of a six-sided top press, placing the six-sided top press, sintering and pressing at 1100 to 1500° C. and 1 to 5 GPa for 10 to 30 minutes, and obtaining a block of reinforced toughened ceramic composite material.

[0008] Preferably, the alcohol aqueous solution is a mixed solution of ethanol and deionized water in a volume ratio of 3:1, and the volume ratio of the silane coupling agent to the alcohol aqueous solution is 1:10-100.

[0009] Preferably, the silane coupling agent is tetraethyl orthosilicate (TEOS).

[0010] Preferably, the nickel-plated PAN-based carbon fiber is a 100-mesh nickel-plated polyacrylonitrile-based (PAN) carbon fiber, and the thickness of the nickel layer is 1.0 to 1.5 um.

[0011] Preferably, the mass ratio of the nano silicon powder to the carbon fiber is 1:5-20, and the thickness of the amorphous silicon oxide film is greater than 10 μm.

[0012] Beneficial effects:

[0013] The present invention adopts a nickel-plated PAN-based carbon fiber whose surface is modified by ethyl orthosilicate to sinter on a six-sided top press to prepare a reinforced and toughened ceramic composite material. A layer of amorphous silicon oxide gel film with uniform thickness and containing nano silicon powder is coated on the surface of the nickel-plated carbon fiber by a sol-gel method to form a Ni-Si-SiO 2 The composite coating increases the number and roughness of active sites on the carbon fiber surface, improves the dispersion and surface wettability of the material, and especially improves the interfacial bonding strength between the carbon fiber and the silicon oxide-based ceramic matrix, giving full play to the high strength and high modulus reinforcement and toughening advantages of carbon fiber in composite materials. The HTHP technology is used to introduce a high-pressure driving force, which can reduce the sintering temperature from the traditional normal pressure process >1700℃ to 1100℃, saving energy, shortening the preparation time, and improving production efficiency. Adding nano-silicon powder particles can inhibit grain growth during the synthesis process, refine the sintered structure, and improve the structure performance. After high temperature and high pressure treatment, the nano-silicon powder combines with the active oxygen in the gel film to form a new chemical bond, and the generated SiO 2 The in-situ growth / crystallization with the amorphous silicon oxide in the gel film, together with the atomic nickel that diffuses to the grain boundaries of the silicon oxide particles through long-range migration under high temperature and high pressure conditions, forms a densely woven cross-linked network of ceramic crystals, which effectively improves the density and toughness of the material. At the same time, the addition of nano-silicon powder can flexibly and conveniently adjust the coating thickness to adjust the quantitative ratio of the silicon oxide matrix ceramic phase, and increase the number of heterogeneous nucleation cores in the crystallization process, which plays a role in refining the grains, and can obtain a fine organization with nano-grains as the overall structure, further improving the toughness and temperature resistance of the ceramic composite material. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 1 is the XRD diagram of the ceramic composite material before and after HTHP sintering in Example 1.

[0015] Figure 2 This is the SEM image of the fracture of the ceramic composite material in Example 1. DETAILED DESCRIPTION

[0016] Example 1

[0017] 5mL of ethyl orthosilicate was added to a mixed solution of 200mL of ethanol and deionized water in a volume ratio of 3:1, and hydrolyzed on a magnetic stirrer at 50°C for 2 hours, and 2g of 300-mesh nickel-plated PAN-based carbon fiber and 0.2g of nano-silicon powder were added, and finally reacted on a magnetic stirrer at 90°C for 4 hours, and then filtered and dried to obtain nickel-plated PAN-based carbon fiber with non-metallic surface modification. It was installed in the assembly block of a six-sided top press, and the assembly block was placed in the six-sided top press, sintered and pressed for 20 minutes at a pressure of 5GPa and a temperature of 1100°C to prepare a ceramic composite material.

[0018] Figure 1 This is the X-ray diffraction (XRD) spectrum of the phase structure of the prepared sintered sample. It can be seen that the diffraction peak of elemental Si in the sample almost completely disappears after sintering, and α-SiO 2 The diffraction peaks indicate that most of the Si element participates in the reaction, combines with the free oxygen groups in the gel film to form silicon oxide, and undergoes crystallization transformation under high temperature and high pressure together with the amorphous silicon oxide generated in situ in the gel film. This process greatly increases the number of heterogeneous nucleation cores and refines the structure of the ceramic composite material. Figure 2 This is a scanning electron microscope (SEM) image of the cross section of the prepared sintered sample. It can be observed that the material grains are at the nanometer level and the fracture characteristics are ductile fracture.

[0019] Example 2

[0020] 3mL of ethyl orthosilicate was added to 200mL of a mixed solution of ethanol and deionized water in a volume ratio of 3:1, and hydrolyzed on a magnetic stirrer for 2 hours at 50°C, and 2g of 300-mesh nickel-plated PAN-based carbon fiber and 0.1g of nano-silicon powder were added. Finally, the reaction was carried out on a magnetic stirrer at 80°C for 5 hours, and then filtered and dried to obtain nickel-plated PAN-based carbon fiber with surface non-metallic modification. The carbon fiber was installed in the assembly block of a six-sided top press, and the assembly block was placed in the six-sided top press. The ceramic composite material was sintered and pressed for 20 minutes under a pressure of 4GPa and a temperature of 1250°C. The cross-sectional morphology of the composite material was observed under a scanning electron microscope. The interface bonding effect between the carbon fiber and the ceramic matrix was good, there were no obvious cracks and holes, the grain size of the organization was fine, and a typical toughness fracture characteristic was presented. The composite material had good toughness and strength.

[0021] Example 3

[0022] 5mL of ethyl orthosilicate was added to a mixed solution of 200mL of ethanol and deionized water in a volume ratio of 3:1, and hydrolyzed on a magnetic stirrer for 4 hours at 50°C, and 2g of 300-mesh nickel-plated PAN-based carbon fiber and 0.4g of nano-silicon powder were added. Finally, the reaction was carried out on a magnetic stirrer at 70°C for 6 hours, and then filtered and dried to obtain nickel-plated PAN-based carbon fiber with non-metallic surface modification. The carbon fiber was installed in the assembly block of a six-sided top press, and the assembly block was placed in the six-sided top press. The ceramic composite material was sintered and pressed for 25 minutes under a pressure of 3GPa and a temperature of 1350°C to prepare the ceramic composite material. The cross-sectional morphology of the composite material was observed under a scanning electron microscope. The interface bonding effect between the carbon fiber and the ceramic matrix was good, there were no obvious cracks and holes, the grain size of the organization was fine, and the typical toughness fracture characteristics were presented. The composite material had good toughness and strength.

[0023] Example 4

[0024] 5mL of ethyl orthosilicate was added to a mixed solution of 200mL of ethanol and deionized water in a volume ratio of 3:1, and hydrolyzed on a magnetic stirrer for 4 hours at 50°C, and 2g of 300-mesh nickel-plated PAN-based carbon fiber and 0.05g of nano-silicon powder were added. Finally, the reaction was carried out on a magnetic stirrer at 60°C for 8 hours, and then filtered and dried to obtain nickel-plated PAN-based carbon fiber with surface non-metallic modification. The carbon fiber was installed in the assembly block of a six-sided top press, and the assembly block was placed in the six-sided top press. The ceramic composite material was sintered and pressed for 30 minutes under a pressure of 2GPa and a temperature of 1400°C to prepare the ceramic composite material. The cross-sectional morphology of the composite material was observed under a scanning electron microscope. The interface bonding effect between the carbon fiber and the ceramic matrix was good, there were no obvious cracks and holes, the grain size of the organization was fine, and the typical toughness fracture characteristics were presented. The composite material had good toughness and strength.

[0025] Example 5

[0026] 5mL of ethyl orthosilicate was added to a mixed solution of 200mL of ethanol and deionized water in a volume ratio of 3:1, and hydrolyzed on a magnetic stirrer at 50°C for 2 hours, and 2g of nickel-plated PAN-based carbon fiber with a specification of 300 mesh and 0.2g of nano-silicon powder were added. Finally, the reaction was carried out on a magnetic stirrer at 50°C for 8 hours, and then filtered and dried to obtain nickel-plated PAN-based carbon fiber with surface non-metallic modification. It was installed in the assembly block of a six-sided top press, and the assembly block was placed in the six-sided top press. It was sintered and pressed for 10 minutes under a pressure of 1GPa and a temperature of 1500°C to prepare a ceramic composite material. The cross-sectional morphology of the composite material was observed under a scanning electron microscope. The interface bonding effect between the carbon fiber and the ceramic matrix was good, there were no obvious cracks and holes, the grain size of the organization was fine, and it showed typical toughness fracture characteristics. The composite material had good toughness and strength.

[0027] In addition to the above benefits, the present invention also innovatively proposes a method for toughening composite materials, namely: by adding nanoparticles and growing them in situ during the synthesis process to become part of the material matrix. At the same time, the thermal strength of the ceramic matrix material synthesized by HTHP technology will be significantly improved, and its temperature resistance under dry friction conditions can exceed 1200°C. On this basis, new superhard material products such as high-temperature resistant abrasive tools with superhard abrasives such as diamond / boron nitride as hard phases can be further prepared. In summary, carbon fiber with surface composite coating treatment is used as a toughening agent, coated silicon oxide is used as a ceramic matrix, and hard particle phases such as diamond, boron nitride, and silicon nitride can be further added. Through high temperature and high pressure technical means, a reinforced and toughened ceramic composite material with high strength, toughness, wear resistance, and high temperature resistance can be prepared.

Claims

1. A high-temperature and high-pressure preparation method for a carbon fiber reinforced toughened ceramic composite material, comprising the following specific steps: adding a silane coupling agent to an alcohol aqueous solution, stirring continuously for 2 to 12 hours at 40 to 100° C., adding nickel-plated PAN-based carbon fiber and nano silicon powder after sufficient hydrolysis, stirring continuously for 2 to 12 hours at 40 to 100° C., filtering and drying the solution after the reaction is completed to obtain nano amorphous silicon oxide coated modified carbon fiber, installing the obtained modified carbon fiber in an assembly block of a six-sided top press, placing the six-sided top press, sintering and pressing at 1100 to 1500° C. and 1 to 5 GPa for 10 to 30 minutes, and obtaining a block of reinforced toughened ceramic composite material.

2. The high temperature and high pressure preparation method of a carbon fiber reinforced toughened ceramic composite material according to claim 1, characterized in that: The alcohol aqueous solution is a mixed solution of ethanol and deionized water in a volume ratio of 3:1, and the volume ratio of the silane coupling agent to the alcohol aqueous solution is 1:10-100.

3. The high temperature and high pressure preparation method of a carbon fiber reinforced toughened ceramic composite material according to claim 1, characterized in that: The silane coupling agent is tetraethyl orthosilicate.

4. The high temperature and high pressure preparation method of a carbon fiber reinforced toughened ceramic composite material according to claim 1, characterized in that: The nickel-plated PAN-based carbon fiber is a 100-mesh nickel-plated polyacrylonitrile-based carbon fiber, and the thickness of the nickel layer is 1.0-1.5 um.

5. The high temperature and high pressure preparation method of a carbon fiber reinforced toughened ceramic composite material according to claim 1, characterized in that: The mass ratio of the nano silicon powder to the carbon fiber is 1:5-20, and the thickness of the amorphous silicon oxide film is greater than 10 μm.

Citation Information

Patent Citations

  • High-temperature and high-pressure preparation method of nickel-plated carbon fiber / silicon oxide composite material

    CN117326880A

  • Preparation process of carbon-carbon composite material with high-temperature stability

    CN117735993A

  • Highly functional composite material and process for producing the same

    WO2007029588A1

Cited By

  • Ceramic particle reinforced wear-resistant alloy material and preparation method thereof