Porous ceramic material, preparation method thereof and honeycomb ceramic heat accumulator

By introducing components such as magnesium aluminum silicate and metal salt into porous ceramic materials to form a protective layer, the problem of poor thermal shock resistance of traditional porous ceramic materials is solved, and a honeycomb ceramic heat storage body with high flexural strength and long life is achieved.

CN118908747AActive Publication Date: 2024-11-08SONGSHAN LAKE MATERIALS LAB +1
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN202411079824.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-08
Estimated Expiration
2044-08-07

AI Technical Summary

Technical Problem

The poor thermal shock resistance of traditional porous ceramic materials leads to significantly increase the loss of flexural strength and shorten the service life.

Method used

Porous ceramic materials, including porous ceramic matrix and protective layer covering it, are prepared by raw materials such as talc and kaolin, combined with components such as magnesium aluminum silicate, sol and metal salt to form a magnesium/aluminum-rich protective layer to improve heat resistance The mass fraction of the protective layer is controlled between 25% and 40% to enhance thermal shock resistance.

Benefits of technology

It significantly improves the thermal shock resistance of porous ceramic materials, reduces the flexural strength loss rate, extends service life, and maintains good heat storage performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908747A_ABST
    Figure CN118908747A_ABST
Patent Text Reader

Abstract

The invention relates to a porous ceramic material, a preparation method thereof and a honeycomb ceramic heat accumulator. The porous ceramic material comprises a porous ceramic matrix and a protective layer coating the porous ceramic matrix, and the mass fraction of the protective layer in the porous ceramic material is 25%-40%; the porous ceramic matrix comprises the following raw materials: talc, kaolin, a first additive, a second additive, a binder, a pore-forming agent, a first dispersant, a lubricant and water; the protective layer is prepared from the following raw materials: magnesium aluminum silicate, sol, metal salt, a second dispersing agent and water; the first additive comprises an aluminum source and / or a silicon source; the second additive comprises mullite whiskers and / or silicon carbide fibers; the metal salt comprises magnesium salt and / or aluminum salt; in the protective layer, the molar ratio of magnesium to aluminum to silicon is 1: (0.5-5): (0.5-4). The porous ceramic material provided by the invention has good heat storage performance and excellent thermal shock resistance, the breaking strength loss rate can be effectively reduced, and the service life is greatly prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of heat storage materials, and in particular to a porous ceramic material and a preparation method thereof, and a honeycomb ceramic heat storage body. Background Art

[0002] Honeycomb ceramic thermal storage body is a key component of thermal storage burner, which is widely used in industrial heat treatment equipment, such as high temperature kilns in industries such as steel smelting, non-ferrous metal smelting and coal-fired power generation, as well as waste gas treatment equipment in industries such as petrochemical, electronic and electrical, and textile printing. In order to promote the role of honeycomb ceramic thermal storage body in energy conservation and emission reduction, the honeycomb ceramic thermal storage body is required to have high temperature resistance, high thermal shock resistance, high structural strength, high heat storage capacity and high heat transfer performance.

[0003] Honeycomb ceramic thermal storage bodies are usually made of porous ceramic materials with high heat capacity and have a honeycomb-like porous structure, which allows a large amount of heat energy to be stored and released quickly, thereby achieving efficient use of heat energy. However, traditional porous ceramic materials have poor thermal shock resistance, resulting in a significant increase in their flexural strength loss and a serious shortening of their service life. Summary of the invention

[0004] Based on this, it is necessary to provide a porous ceramic material and a preparation method thereof and a honeycomb ceramic thermal storage body to overcome the problem that traditional porous ceramic materials have poor thermal shock resistance, resulting in significantly increased loss of flexural strength and severely shortened service life.

[0005] The above-mentioned purpose of the present application is achieved through the following technical solutions:

[0006] In a first aspect of the present application, a porous ceramic material is provided, comprising a porous ceramic substrate and a protective layer covering the porous ceramic substrate, wherein the mass fraction of the protective layer in the porous ceramic material is 25% to 40%;

[0007] The raw materials of the porous ceramic matrix include talc, kaolin, a first additive, a second additive, a binder, a pore former, a first dispersant, a lubricant and water;

[0008] The raw materials of the protective layer include magnesium aluminum silicate, sol, metal salt, a second dispersant and water;

[0009] Wherein, the first additive comprises one or more of an aluminum source and a silicon source;

[0010] The second additive includes one or more of mullite whiskers and silicon carbide fibers;

[0011] The metal salt includes one or more of a magnesium salt and an aluminum salt;

[0012] In the protective layer, the molar ratio of magnesium element, aluminum element and silicon element is 1:(0.5-5):(0.5-4).

[0013] In one embodiment, the porous ceramic matrix comprises the following raw materials in parts by weight:

[0014] .

[0015] In one embodiment, the protective layer comprises the following raw materials in parts by weight:

[0016] .

[0017] In one embodiment, the aluminum source includes one or more of aluminum oxide, aluminum hydroxide and bauxite.

[0018] In one embodiment, the silicon source includes one or more of silicon powder, quartz sand and yellow sand.

[0019] In one of the embodiments, in the first additive, the mass ratio of the aluminum source to the silicon source is (0-15):(0-10), and the masses of the aluminum source and the silicon source are not zero at the same time.

[0020] In one embodiment, in the second additive, the mass ratio of the mullite whisker to the silicon carbide fiber is (0-15):(0-10), and the masses of the mullite whisker and the silicon carbide fiber are not zero at the same time.

[0021] In one embodiment, the binder includes a cellulose-based binder.

[0022] In one embodiment, the pore former includes one or more of an inorganic carbon material and an organic carbon material.

[0023] In one embodiment, the first dispersant and the second dispersant independently include one or more of oleic acid, sodium oleate, potassium oleate, triethanolamine oleate, polyoxyethylene nonylphenol ether-9 and dodecyltrimethylammonium chloride.

[0024] In one embodiment, the lubricant includes one or more of vegetable oil and mineral oil.

[0025] In one embodiment, the magnesium salt includes one or more of magnesium hydroxide, magnesium carbonate, magnesium silicate and magnesium phosphate.

[0026] In one embodiment, the aluminum salt includes one or more of aluminum hydroxide, aluminum dihydrogen phosphate, aluminum silicate and aluminum nitrate.

[0027] In one embodiment, in the metal salt, the mass ratio of the magnesium salt to the aluminum salt is (0-5):(0-10), and the masses of the magnesium salt and the aluminum salt are not zero at the same time.

[0028] In one embodiment, the sol includes one or more of silica sol, aluminum sol, zirconium sol and titanium sol.

[0029] In a second aspect of the present application, there is provided a method for preparing the porous ceramic material as described above, comprising the following steps:

[0030] Mixing talc, kaolin, a first additive, a second additive, a binder, a pore former, a first dispersant, a lubricant and water, and performing mud kneading, aging, mud refining, extrusion molding, first drying and first calcination to prepare a porous ceramic matrix;

[0031] Wetting the porous ceramic substrate with water vapor to prepare a pretreated substrate;

[0032] The pre-treated substrate is impregnated with a suspension containing magnesium aluminum silicate, sol, metal salt, a second dispersant and water, and purged, second dried and second calcined to form a protective layer on the pre-treated substrate.

[0033] In one embodiment, the wetting process comprises the following steps:

[0034] The porous ceramic substrate is wetted by water vapor at a temperature of 110° C. to 150° C. and a pressure of 40 Pa to 380 Pa, and the wetting time is 2 min to 5 min.

[0035] In one embodiment, the first drying method and the second drying method each independently comprise microwave drying.

[0036] In one embodiment, the first calcination comprises the following steps:

[0037] Raise the temperature to 1300℃~1440℃ at a heating rate of 150℃ / h~300℃ / h and keep it at this temperature for 4h~10h.

[0038] In one embodiment, the second calcination comprises the following steps:

[0039] Raise the temperature to 1250℃~1400℃ at a heating rate of 100℃ / h~200℃ / h and keep it at this temperature for 3h~6h.

[0040] In a second aspect of the present application, a honeycomb ceramic heat storage body is provided, which is made of the porous ceramic material as described above, or a porous ceramic material prepared by the method for preparing the porous ceramic material as described above.

[0041] In one embodiment, the heat resistance loss rate of the honeycomb ceramic thermal storage body is ≤2.5%.

[0042] In one embodiment, the apparent porosity of the honeycomb ceramic thermal storage body is 1.78% to 12.2%.

[0043] In one embodiment, the thermal conductivity of the honeycomb ceramic thermal storage body is 1.5W / (m·℃)~1.8W / (m·℃).

[0044] This application has at least the following beneficial effects:

[0045] The present application uses talc and kaolin as main raw materials, utilizes a first additive to balance the content of aluminum and silicon, utilizes a second additive as a reinforcing agent to enhance the mechanical strength of the matrix, utilizes a pore-forming agent to cause the matrix to form a porous structure rich in pores, and utilizes a combination and matching of a binder, a first dispersant, and a lubricant to ensure the uniformity, plasticity, and fluidity of the mud material, thereby obtaining a porous ceramic matrix with good heat storage performance, high porosity, and high thermal shock resistance.

[0046] At the same time, the present application uses magnesium aluminum silicate as an inorganic gel thickener, which, in combination with the sol and the second dispersant, can promote the formation of a firm and tight bond between the protective layer and the substrate, and adjust the component content and uniformity of the protective layer to avoid the protective layer and the substrate from falling off due to excessive differences in composition; the metal salt is used to adjust the molar ratio of the three elements of magnesium, aluminum and silicon in the protective layer, and form a magnesium / aluminum-rich protective layer on the pores and outer walls of the substrate, fill and repair defects such as tiny cracks and voids on the surface of the substrate, effectively reduce the stress concentration generated under the action of thermal shock cycles, avoid cracking, peeling and other thermal shock damage, thereby significantly improving the thermal shock resistance of porous ceramic materials; the mass fraction of the protective layer is controlled at 25% to 40%, while enhancing the thermal shock resistance, it will not block the pores of the substrate. Therefore, the porous ceramic material provided by the present application has both good thermal storage performance and excellent thermal shock resistance, can effectively reduce the flexural strength loss rate, and greatly extend the service life, and is very suitable for making honeycomb ceramic thermal storage bodies. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] In order to more clearly illustrate the technical solutions in the embodiments of the present application and to more completely understand the present application and its beneficial effects, the following is a brief introduction to the drawings required for the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present application, and those skilled in the art can obtain other drawings based on these drawings without creative work.

[0048] Figure 1 This is a physical picture of the porous ceramic material obtained in Example 1;

[0049] Figure 2 for Figure 1 A left side view of the porous ceramic material shown;

[0050] Figure 3 for Figure 1 A top view of the porous ceramic material is shown. DETAILED DESCRIPTION

[0051] In order to facilitate the understanding of the present application, the present application is further described in detail below in conjunction with specific embodiments. However, the present application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present application more thorough and comprehensive.

[0052] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.

[0053] In the present application, the meaning of "and / or" includes any and all combinations of one or more related listed items. "At least one" means more than one, such as one, two and more than two. "Multiple" or "several" means at least two, such as two, three, etc., and "multi-layer" means at least two layers, such as two layers, three layers, etc., unless otherwise clearly and specifically defined. In the description of the present application, "several" means at least one, such as one, two, etc., unless otherwise clearly and specifically defined.

[0054] When a numerical range is disclosed in this application, the above range is considered to be continuous and includes the minimum and maximum values ​​of the range, as well as every value between such minimum and maximum values. Further, when a range refers to an integer, every integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be combined. In other words, unless otherwise indicated, all ranges disclosed in this application should be understood to include any and all subranges included therein.

[0055] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may also include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0056] In this application, "above" or "below" includes the number itself. For example, "1 below" includes 1.

[0057] The temperature parameters in this application, unless otherwise specified, are allowed to be either constant temperature treatment or to vary within a certain temperature range. It should be understood that the constant temperature treatment allows the temperature to fluctuate within the accuracy range controlled by the instrument. Fluctuations within the range of ±5°C, ±4°C, ±3°C, ±2°C, and ±1°C are allowed.

[0058] In the present application, room temperature refers to indoor temperature, normal temperature or general temperature. Generally speaking, the range of room temperature can be any one of the following temperature intervals: 23°C ± 2°C, 25°C ± 5°C or 20°C ± 5°C.

[0059] the term

[0060] Unless otherwise specified or incompatible herewith, the terms and phrases used herein shall have the following meanings:

[0061] Thermal shock resistance: refers to the ability of a material to maintain its structure and performance without significant changes under high temperature. Under high temperature regulation, the material will produce thermal expansion and contraction due to temperature changes, which is easy to cause stress concentration and thermal cracks, thus affecting the service life and safety of the material.

[0062] Flexural strength: Flexural strength refers to the material's ability to resist bending when subjected to stress, that is, the material's ability to resist bending without breaking when subjected to bending force. It is usually called flexural strength. It is mainly used to measure the strength of brittle materials such as ceramics. The unit is megapascal (MPa).

[0063] Flexural strength loss rate: refers to the degree of reduction in the flexural strength of a material before and after it is subjected to force. The smaller the flexural strength loss rate, the better the thermal shock resistance of the material.

[0064] Honeycomb ceramic heat storage bodies are usually made of porous ceramic materials with high heat capacity, but the thermal shock resistance of traditional porous ceramic materials is relatively low, which leads to alternating stress in the heat storage body during long-term operation due to frequent heat storage, heat release and cooling processes, thus forming cracks on the outer wall and the pore wall, causing the pores to be blocked, or even ruptured or collapsed. When the pores of the heat storage body are blocked or crushed, it will not only cause an increase in the loss of flexural strength, but also greatly shorten the service life.

[0065] Based on this, in the first aspect of the present application, a porous ceramic material is provided.

[0066] Optionally, the porous ceramic material includes a porous ceramic matrix and a protective layer covering the porous ceramic matrix, and the mass fraction of the protective layer in the porous ceramic material is 25% to 40%;

[0067] The raw materials of the porous ceramic matrix include talc, kaolin, a first additive, a second additive, a binder, a pore former, a first dispersant, a lubricant and water;

[0068] The raw materials of the protective layer include magnesium aluminum silicate, sol, metal salt, second dispersant and water;

[0069] Wherein, the first additive includes one or more of an aluminum source and a silicon source;

[0070] The second additive includes one or more of mullite whiskers and silicon carbide fibers;

[0071] The metal salt includes one or more of a magnesium salt and an aluminum salt;

[0072] In the protective layer, the molar ratio of magnesium, aluminum and silicon is 1:(0.5~5):(0.5~4).

[0073] The present application uses talc and kaolin as main raw materials, utilizes a first additive to balance the content of aluminum and silicon, utilizes a second additive as a reinforcing agent to enhance the mechanical strength of the matrix, utilizes a pore-forming agent to cause the matrix to form a porous structure rich in pores, and utilizes a combination and matching of a binder, a first dispersant, and a lubricant to ensure the uniformity, plasticity, and fluidity of the mud material, thereby obtaining a porous ceramic matrix with good heat storage performance, high porosity, and high thermal shock resistance.

[0074] At the same time, the present application uses magnesium aluminum silicate as an inorganic gel thickener, which cooperates with the sol and the second dispersant to promote a firm and tight bond between the protective layer and the substrate, and adjusts the component content and uniformity of the protective layer to avoid the protective layer and the substrate from falling off due to excessive differences in composition; the metal salt is used to adjust the molar ratio of the three elements of magnesium, aluminum and silicon in the protective layer, and to form a magnesium / aluminum-rich protective layer on the pores and outer walls of the substrate, filling and repairing defects such as tiny cracks and voids on the surface of the substrate, effectively reducing the stress concentration generated under the action of thermal shock cycles, avoiding thermal shock damage such as cracking and peeling, thereby significantly improving the thermal shock resistance of the porous ceramic material; the mass fraction of the protective layer is controlled at 25%~40%, and the pores of the substrate will not be blocked while enhancing the thermal shock resistance. Therefore, the porous ceramic material provided by the present application has both good thermal storage performance and excellent thermal shock resistance, can effectively reduce the flexural strength loss rate, and greatly extend the service life, and is very suitable for making honeycomb ceramic thermal storage bodies.

[0075] It can be understood that magnesium aluminum silicate, as an inorganic gel thickener, can form a highly thixotropic inorganic gel in an aqueous solution with its unique lamellar structure, and has an excellent dispersing effect, preventing other raw materials from flocculating, stratifying and settling, forming a uniform and stable suspension system, thereby improving the uniformity of the composition and thickness of the protective layer. At the same time, magnesium aluminum silicate can also introduce a certain amount of silicon, magnesium and aluminum elements into the protective layer, which can not only enhance the thermal shock resistance, but also reduce the composition difference between the protective layer and the substrate, and prevent the protective layer from falling off.

[0076] As an example, the mass fraction of the protective layer in the porous ceramic material can be 25%, 26%, 27%, 28%, 29%, 30%, 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38%, 39% or 40%.

[0077] As an example, in the protective layer, the molar ratio of magnesium element to aluminum element can be 1:0.5, 1:1, 1:1.5, 1:2, 1:2.5, 1:3, 1:3.5, 1:4, 1:4.5 or 1:5.

[0078] As an example, in the protective layer, the molar ratio of magnesium element to silicon element may be 1:0.5, 1:1, 1:1.5, 1:2, 1:2.5, 1:3, 1:3.5 or 1:4.

[0079] Optionally, the porous ceramic matrix includes the following raw materials in parts by weight:

[0080] .

[0081] As an example, in the raw materials of the porous ceramic matrix, the weight portion of talc can be 35 parts, 36 parts, 37 parts, 38 parts, 39 parts, 40 parts, 41 parts or 42 parts; the weight portion of kaolin can be 20 parts, 25 parts, 30 parts, 35 parts, 40 parts, 45 parts, 50 parts, 55 parts, 60 parts, 65 parts or 70 parts, and can be further selected as 32 parts to 50 parts; the weight portion of the first additive can be 5 parts, 8 parts, 10 parts, 12 parts, 15 parts, 18 parts, 20 parts, 22 parts, 24 parts or 25 parts; the weight portion of the second additive can be 5 parts, 8 parts, 10 parts, 12 parts, 15 parts, 18 parts, 20 parts, 22 parts, 24 parts or 25 parts; the weight portion of the binder can be 1.2 parts, 1.5 parts , 1.8, 2, 2.5, 3, 3.4, 4, 4.5 or 5 parts by weight; the weight portion of the pore-forming agent can be 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14 or 15 parts; the weight portion of the first dispersant can be 1, 1.5, 2, 2.5, 3, 3.4, 4, 4.5 or 5 parts; the weight portion of the lubricant can be 0.5, 0.8, 1, 1.2, 1.5, 1.8, 2, 2.2, 2.5, 2.8 or 3 parts; the weight portion of water can be 20, 21, 22, 23, 24, 25, 26, 27, 28, 29 or 30 parts.

[0082] Optionally, the protective layer comprises the following raw materials in parts by weight:

[0083] .

[0084] As an example, in the raw material of the protective layer, the weight parts of magnesium aluminum silicate can be 15 parts, 16 parts, 17 parts, 18 parts, 19 parts, 20 parts, 21 parts, 22 parts, 23 parts, 24 parts, 25 parts, 26 parts, 27 parts, 28 parts, 29 parts or 30 parts; the weight parts of sol can be 15 parts, 16 parts, 17 parts, 18 parts, 19 parts, 20 parts, 21 parts, 22 parts, 23 parts, 24 parts, 25 parts, 26 parts, 27 parts, 28 parts, 29 parts or 30 parts; the weight parts of the metal salt can be The weight parts of the second dispersant can be 2, 2.2, 2.5, 2.8, 3, 3.2, 3.5, 3.8, 4, 4.2, 4.5, 4.8 or 5 parts; the weight parts of water can be 50, 55, 60, 65, 70, 75, 80, 85 or 90 parts.

[0085] It can be understood that talc has good thermal conductivity and high heat capacity, and kaolin has excellent thermal conductivity and thermal stability. The combination of talc and kaolin can improve the thermal conductivity, heat capacity and thermal stability of the matrix, thereby achieving efficient use of thermal energy.

[0086] Optionally, the kaolin includes one or more of washed kaolin and calcined kaolin. Further optionally, the kaolin is washed kaolin, and calcined kaolin is not added; or, the kaolin is a combination of washed kaolin and calcined kaolin, and the mass ratio of washed kaolin to calcined kaolin is (1-2):1. As an example, the mass ratio of washed kaolin to calcined kaolin can be 1:1, 1.1:1, 1.2:1, 1.4:1, 1.6:1, 1.8:1 or 2:1.

[0087] Understandably, water washing and calcination are common treatment methods for natural kaolin. Among them, water-washed kaolin is to wash natural kaolin with water to remove impurities and organic matter and improve purity and whiteness. Calcined kaolin is to calcine natural kaolin at high temperature to change its crystal structure and increase the grain size, thereby improving its fire resistance, bonding and corrosion resistance. However, using calcined kaolin alone will significantly reduce the plasticity of the mud, which is not conducive to extrusion molding. Therefore, water-washed kaolin is usually used as the main material, and a small amount of calcined kaolin is added as an auxiliary material.

[0088] In the present application, the first additive is used to adjust the composition of the matrix and balance the content of aluminum and silicon to obtain better thermal shock resistance. There is no particular restriction on the type and amount of the first additive. According to the performance requirements and application scenarios of the porous ceramic material, an appropriate amount of aluminum source or silicon source can be added to make it have both excellent heat storage performance and good thermal shock resistance.

[0089] Optionally, the aluminum source includes one or more of aluminum oxide (Al2O3), aluminum hydroxide (Al(OH)3) and bauxite, further optionally aluminum oxide, and further optionally calcined aluminum oxide.

[0090] Optionally, the silicon source includes one or more of silicon micropowder, quartz sand and yellow sand, and further silicon micropowder can be selected. Yellow sand (or yellow sand) is common sand for construction, the main component of which is silicon dioxide, but the impurity content is higher than that of quartz sand.

[0091] Optionally, in the first additive, the mass ratio of the aluminum source to the silicon source is (0-15):(0-10), and the masses of the aluminum source and the silicon source are not zero at the same time. Further optionally, the first additive is an aluminum source, and no silicon source is added; or, the first additive is a silicon source, and no aluminum source is added; or, the first additive includes an aluminum source and a silicon source, and the mass ratio of the aluminum source to the silicon source is (2-15):(3-10). As an example, the mass ratio of the aluminum source to the silicon source can be 2:3, 2:5, 2:8, 2:10, 5:3, 5:5, 5:8, 5:10, 10:3, 10:5, 10:8, 15:3, 15:5, 15:8 or 15:10.

[0092] In the present application, the second additive is mainly used as a reinforcing agent to enhance the intrinsic mechanical strength of the porous ceramic matrix. There is no particular restriction on its type and amount. According to the performance requirements and application scenarios of the porous ceramic material, an appropriate amount of mullite whiskers or silicon carbide fibers can be added to make it exhibit higher thermal shock resistance.

[0093] Optionally, in the second additive, the mass ratio of mullite whisker to silicon carbide fiber is (0~15):(0~10), and the mass of mullite whisker and silicon carbide fiber are not zero at the same time. Further optionally, the second additive is mullite whisker, and silicon carbide fiber is not added; or, the second additive is silicon carbide fiber, and mullite whisker is not added; or, the second additive includes mullite whisker and silicon carbide fiber, and the mass ratio of mullite whisker to silicon carbide fiber is (3~15):(5~10). As an example, the mass ratio of mullite whisker to silicon carbide fiber can be 3:5, 3:8, 3:10, 5:5, 5:8, 5:10, 10:5, 10:8, 15:5, 15:8 or 15:10.

[0094] In the present application, the pore former will undergo thermal decomposition during high-temperature sintering and be converted into volatile gas, which will cause the matrix to form a porous structure rich in pores, thereby enhancing the thermal conductivity and heat dissipation performance of the porous ceramic material.

[0095] Optionally, the pore-forming agent includes one or more of an inorganic carbon material and an organic carbon material. Among them, the inorganic carbon material includes one or more of graphite, graphite oxide, graphene, carbon fiber, and carbon nanotubes; the organic carbon material includes one or more of glucose, fructose, maltose, cellulose, starch, modified starch, and polymer microspheres; the polymer microspheres include one or more of polystyrene (PS) microspheres, polymethyl methacrylate (PMMA) microspheres, polyvinyl chloride (PVC) microspheres, polyethyleneimine (PEI) microspheres, and polylactic acid (PLA) microspheres. Further, one or more of graphite, graphite oxide, starch, modified starch, and polyethylene microspheres can be selected. Further, one or more of graphite and graphite oxide can be selected.

[0096] In the present application, the reasonable combination and matching of the binder, the first dispersant and the lubricant ensures the uniformity of dispersion of the raw materials, effectively avoids particle accumulation, improves the plasticity and fluidity of the mud, reduces the extrusion pressure and molding pressure, reduces the irreversible wear of the mold and equipment, and is beneficial to the extrusion molding and high-temperature sintering of the mud.

[0097] Optionally, the binder includes a cellulose binder, wherein the cellulose binder includes one or more of methyl cellulose, ethyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, carboxymethyl cellulose, hydroxypropyl cellulose ether and hydroxypropyl methyl cellulose, and further methyl cellulose may be selected.

[0098] Optionally, the first dispersant and the second dispersant each independently include one or more of oleic acid, sodium oleate, potassium oleate, triethanolamine oleate, polyoxyethylene nonylphenol ether and dodecyltrimethylammonium chloride, and potassium oleate may further be selected.

[0099] Understandably, oleic acid, oleate and oleic acid derivatives contain hydrophilic and hydrophobic groups in their structures, which can interact with water and oil, thereby reducing surface tension and having excellent dispersing and emulsifying abilities. Polyoxyethylene Nonyl Phenol Ether-9 (NP-9) is a nonionic surfactant that contains a nonylphenol group and multiple ethylene oxide units in its structure. It has good surface activity and wetting properties and can emulsify and disperse in aqueous and oily systems. Dodecyltrimethylammonium chloride (DTAC) is a quaternary ammonium salt cationic surfactant with good surface activity and emulsifying properties.

[0100] Optionally, the lubricant includes one or more of vegetable oil and mineral oil. The vegetable oil includes one or more of tung oil, soybean oil, castor oil, rapeseed oil and palm oil; the mineral oil includes white oil. Further optionally, the lubricant includes one or more of tung oil and soybean oil.

[0101] In the present application, metal salts are used to form a magnesium / aluminum-rich protective layer on the pores and outer walls of the substrate, and to fill and repair defects such as tiny cracks and voids generated in the substrate during high-temperature sintering, thereby effectively reducing the stress concentration generated by thermal shock cycles, avoiding thermal shock damage such as cracking and spalling, and thus significantly improving the thermal shock resistance of porous ceramic materials.

[0102] Optionally, the magnesium salt includes one or more of magnesium hydroxide (Mg(OH)2), magnesium carbonate (MgCO3), magnesium silicate (MgSiO3) and magnesium phosphate (Mg3(PO4)2), and may further be one or more of magnesium hydroxide and magnesium phosphate.

[0103] Optionally, the aluminum salt includes one or more of aluminum hydroxide (Al(OH)3), aluminum dihydrogen phosphate (Al(H2PO4)3), aluminum silicate (Al2O3·SiO2) and aluminum nitrate (Al(NO3)3), and can further be one or more of aluminum hydroxide and aluminum silicate.

[0104] Optionally, in the metal salt, the mass ratio of magnesium salt to aluminum salt is (0-5): (0-10), and the mass of magnesium salt and aluminum salt are not zero at the same time. Further optionally, the metal salt is a magnesium salt, and no aluminum salt is added; or, the metal salt is an aluminum salt, and no magnesium salt is added; or, the metal salt includes a magnesium salt and an aluminum salt, and the mass ratio of magnesium salt to aluminum salt is (1-5): (1-10). As an example, the mass ratio of magnesium salt to aluminum salt can be 1:1, 1:5, 1:10, 2:1, 2:5, 4:1, 4:5, 5:1 or 5:10.

[0105] In the present application, the sol promotes the formation of a strong bond between the protective layer and the substrate, and can adjust the composition of the protective layer to avoid the protective layer and the substrate from falling off due to a large difference in composition, and also plays a key role in improving thermal shock resistance.

[0106] Optionally, the sol includes one or more of silica sol, aluminum sol, zirconium sol and titanium sol, and further may be one or more of silica sol and aluminum sol.

[0107] Optionally, the water in the raw materials of the porous ceramic substrate and the protective layer independently includes one or more of tap water, deionized water, distilled water, reverse osmosis water, pure water and ultrapure water. Among them, tap water is beneficial to reducing the cost of the porous ceramic material, and deionized water or pure water is beneficial to improving the quality and thermal storage performance of the porous ceramic material.

[0108] In a second aspect of the present application, a method for preparing the porous ceramic material as described above is provided.

[0109] In some embodiments, the method for preparing the porous ceramic material comprises the following steps:

[0110] S100: mixing talc, kaolin, a first additive, a second additive, a binder, a pore former, a first dispersant, a lubricant and water, performing mud kneading, aging, mud refining, extrusion molding, first drying and first calcination to prepare a porous ceramic matrix;

[0111] S200: Wetting the porous ceramic substrate with water vapor to prepare a pretreated substrate;

[0112] S300: The pretreated substrate is impregnated with a suspension containing magnesium aluminum silicate, sol, metal salt, a second dispersant and water, and purged, second dried and second calcined to form a protective layer on the porous ceramic substrate.

[0113] Optionally, the mixing method of the raw materials includes one or more of a stirring method, an ultrasonic method and a ball milling method.

[0114] Optionally, in step S100, the raw materials are mixed by mechanical stirring, such as dry mixing without a solvent and wet mixing with a liquid phase.

[0115] Optionally, in step S300, the method for preparing the suspension includes the following steps: uniformly stirring magnesium aluminum silicate, sol, metal salt, second dispersant and water, and performing ultrasonic dispersion and ball milling. The power of ultrasonic dispersion is 60W~120W, and the time is 0.5h~2.5h; the ball milling time is 12h~48h, the ball milling speed is 300rpm~500rpm, the ball milling medium is deionized water, and the material-ball ratio is (2~3):1.

[0116] Optionally, the wetting treatment includes the following steps: using water vapor with a temperature of 110° C. to 150° C. and a pressure of 40 Pa to 380 Pa to wet the porous ceramic substrate for a wetting time of 2 min to 5 min.

[0117] As an example, water vapor can be provided by a high-temperature superheated water vapor generator; the temperature of the water vapor can be 110°C, 115°C, 120°C, 125°C, 130°C, 135°C, 140°C, 145°C or 150°C; the pressure of the water vapor is 40Pa, 80Pa, 120Pa, 160Pa, 200Pa, 240Pa, 280Pa, 320Pa, 360Pa or 380Pa; the wetting time is 2min, 2.5min, 3min, 3.5min, 4min, 4.5min or 5min.

[0118] The porous ceramic substrate has an extremely low water content and is prone to adsorb a large amount of liquid phase in the suspension during the impregnation process, which significantly increases the viscosity of the suspension and easily causes channel blockage, reducing the load of the protective layer and the coating effect. Through wetting treatment, the wettability of the solid interface such as the surface of the porous ceramic substrate channel, pores and capillaries can be improved, preventing excessive adsorption of the liquid phase in the suspension during the impregnation process, avoiding the blockage of the substrate surface channels, pores and capillaries, thereby increasing the load of the protective layer and improving the coating effect.

[0119] Optionally, the first drying method and the second drying method each independently comprise microwave drying.

[0120] Optionally, in the first drying, the power of microwave drying is 700W-1400W, and the time of microwave drying is 5min-30min. As an example, in the first drying, the power of microwave drying can be 700W, 800W, 900W, 1000W, 1100W, 1200W, 1300W or 1400W.

[0121] Optionally, in the second drying, the power of microwave drying is 350W-1000W, and the time of microwave drying is 5min-10min. As an example, in the second drying, the power of microwave drying can be 350W, 400W, 500W, 600W, 700W, 800W, 900W or 1000W.

[0122] Optionally, the first calcination comprises the following steps: heating to 1300°C-1440°C at a heating rate of 150°C / h-300°C / h, and keeping the temperature for 4h-10h.

[0123] As an example, in the first calcination, the heating rate can be 150℃ / h, 180℃ / h, 210℃ / h, 240℃ / h, 270℃ / h or 300℃ / h, the calcination temperature can be 1300℃, 1320℃, 1340℃, 1360℃, 1380℃, 1400℃, 1420℃ or 1440℃, and the keeping time at the calcination temperature can be 4h, 5h, 6h, 7h, 8h, 9h or 10h.

[0124] Optionally, the second calcination comprises the following steps: heating to 1250°C-1400°C at a heating rate of 100°C / h-200°C / h, and keeping the temperature for 3h-6h.

[0125] As an example, in the second calcination, the heating rate can be 100℃ / h, 120℃ / h, 140℃ / h, 160℃ / h, 180℃ / h or 500℃ / h, the calcination temperature can be 1250℃, 1280℃, 1300℃, 1320℃, 1340℃, 1360℃, 1380℃ or 1400℃, and the keeping time at the calcination temperature can be 3h, 4h, 5h or 6h.

[0126] Optionally, the device for kneading the mud material is a kneading machine, which can be a normal type, a pressure type, a vacuum type or a high temperature type kneading machine, and can further be a vacuum kneading machine.

[0127] Optionally, the aging condition includes the following steps: sealing the kneaded clay material and leaving it at room temperature for 12 hours to 84 hours. In some specific examples, the kneaded clay material is sealed with a plastic film, stored in a cool place indoors, and left at room temperature for 12 hours to 84 hours.

[0128] Optionally, the mud refining equipment adopts a vacuum mud refining machine.

[0129] Optionally, the extrusion molding equipment adopts a vacuum screw extruder.

[0130] Optionally, the method of impregnating the porous ceramic matrix into the suspension is a vacuum impregnation method, wherein in the vacuum impregnation method, the temperature of the suspension is 22° C. to 28° C., the impregnation time is 3 h to 5 h, and the vacuum degree is 0.05 MPa to 0.08 MPa.

[0131] Optionally, the wind speed of the purge is 1.2 m / s to 5.0 m / s, the purge time is 5 s to 10 s, and the purge temperature is room temperature.

[0132] In a third aspect of the present application, a honeycomb ceramic heat storage body is provided, which is made of the porous ceramic material as described above, or a porous ceramic material prepared by the method for preparing the porous ceramic material as described above.

[0133] Optionally, the heat resistance strength loss rate of the honeycomb ceramic thermal storage body is ≤2.5%, for example, 0.1%, 0.2%, 0.5%, 0.8%, 1%, 1.2%, 1.5%, 1.8%, 2%, 2.2% or 2.5%.

[0134] Optionally, the apparent porosity of the honeycomb ceramic thermal storage body is 1.78% to 12.2%, for example, 1.78%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12% or 12.2%.

[0135] Optionally, the thermal conductivity of the honeycomb ceramic thermal storage body is 1.5W / (m·℃)~1.8W / (m·℃), for example, 1.5W / (m·℃), 1.55W / (m·℃), 1.6W / (m·℃), 1.65W / (m·℃), 1.7W / (m·℃), 1.75W / (m·℃) or 1.8W / (m·℃).

[0136] The following is further described in conjunction with specific embodiments and comparative examples. The raw materials involved in the following specific embodiments and comparative examples, unless otherwise specified, can all be commercially available, the instruments used, unless otherwise specified, can all be commercially available, and the processes involved, unless otherwise specified, are all routinely selected by those skilled in the art.

[0137] Example 1

[0138] Please refer to Table 1 and Table 2. The mass ratio of the porous ceramic substrate and the protective layer in this embodiment is 100:(30-35).

[0139] The porous ceramic matrix is ​​composed of the following raw materials in parts by weight: 35 parts of talc, 47 parts of kaolin, 8 parts of the first additive, 8 parts of the second additive, 3 parts of a binder, 4 parts of a pore former, 5 parts of a first dispersant, 2 parts of a lubricant, and 24 parts of water. Among them, the kaolin is composed of 25 parts of washed kaolin and 22 parts of calcined kaolin, the first additive is silicon powder (silicon source), the second additive is mullite whisker, the binder is methyl cellulose, the pore former is graphite fine powder, and the first dispersant is potassium oleate.

[0140] The protective layer is composed of the following raw materials in parts by weight: 20 parts of magnesium aluminum silicate, 15 parts of sol, 10 parts of metal salt, 5 parts of second dispersant and 50 parts of deionized water. Among them, the sol is composed of 5 parts of silica sol and 10 parts of aluminum sol, the metal salt is composed of 5 parts of magnesium phosphate (magnesium salt) and 5 parts of aluminum hydroxide (aluminum salt), and the second dispersant is potassium oleate.

[0141] The preparation method of the porous ceramic material of this embodiment is as follows:

[0142] (1) dry-mixing talc, kaolin, a first additive, a second additive, a binder and a pore-forming agent to obtain a powder; mixing a first dispersant and water to obtain a dispersion; adding the dispersion to the powder for wet mixing to obtain a wet powder; continuously stirring in a mixer until the temperature of the wet powder is greater than 45°C, adding a lubricant and continuing wet mixing to obtain a mud material; kneading, aging and refining the mud material in sequence, and extruding and molding the mud material using a vacuum screw extruder to obtain a wet molded blank; drying the molded material by microwave at 750W for 10 minutes to obtain a dry molded blank with a moisture content of less than 3wt%; then heating the temperature to 1350°C at a heating rate of 200°C / h, and maintaining the highest temperature for 4 hours to obtain a porous ceramic matrix.

[0143] (2) The porous ceramic substrate was wetted using a high-temperature superheated water vapor generator, with the water vapor temperature being controlled at 120°C, the water vapor pressure being controlled at 210 kPa, and the wetting time being controlled at 4 min to obtain a pretreated substrate.

[0144] (3) The magnesium aluminum silicate, sol, metal salt, second dispersant and water are stirred evenly and ultrasonically dispersed, and then placed in a ball mill, and ball milled for 24 hours at a material-to-ball ratio of 2:1, deionized water as the ball milling medium and a ball milling speed of 350 rpm, and cooled to room temperature to obtain a suspension; the pretreated substrate is completely immersed in the suspension, vacuum impregnated for 4.5 hours under the conditions of a vacuum degree of 0.08 MPa and a suspension temperature of 25°C, and then purged for 10 seconds at room temperature and a wind speed of 5.0 m / s to obtain a semi-finished product; the semi-finished product is microwave dried at 550 W for 8 minutes, and then heated to 1250°C at a heating rate of 200°C / h and kept warm for 3 hours, so that a protective layer is formed on the porous ceramic substrate to obtain a porous ceramic material.

[0145] Embodiments 2 to 7

[0146] The formulas of the porous ceramic materials of Examples 2 to 7 are detailed in Tables 1 to 2, and the preparation methods are the same as those of Example 1.

[0147] Comparative Example 1

[0148] The formula of the porous ceramic material of this comparative example is shown in Tables 3-4. The difference between this comparative example and Example 1 is that after the porous ceramic substrate is prepared, steps (2) and (3) are not performed.

[0149] Comparative Example 2

[0150] The formulation of Comparative Example 2 is the same as that of Example 1, but the wetting treatment in step (2) is not performed.

[0151] Comparative Examples 3 to 7

[0152] The formulas of the porous ceramic materials of Comparative Examples 3 to 7 are detailed in Tables 3 to 4, and the preparation methods are the same as those of Example 1.

[0153] Test Example 1

[0154] The porous ceramic material was tested as follows, and the results are shown in Table 5.

[0155] (1) Protective layer loading rate: Use an analytical balance to weigh the mass of the porous ceramic substrate and the mass of the porous ceramic material obtained after wetting and impregnation and other modification treatments, and calculate using the following formula: Protective layer loading rate = (mass of porous ceramic material - mass of porous ceramic substrate) / mass of porous ceramic material × 100%. The protective layer loading rate can be used to determine the mass fraction of the protective layer in the porous ceramic material and the mass ratio of the porous ceramic substrate to the protective layer. For example, a protective layer loading rate of 30% means that the mass fraction of the protective layer in the porous ceramic material is 30%, which means that the mass ratio of the porous ceramic substrate to the protective layer is 70:30.

[0156] (2) Apparent porosity: Tested in accordance with standard HGT3210-2002.

[0157] (3) Thermal conductivity: Tested in accordance with standard GB / T5990-2021.

[0158] (4) Flexural strength loss rate: The flexural strength of ceramic materials was measured using a material surface and interface performance tester, and the flexural strength loss rate of porous ceramic materials after 30 thermal shock cycles from room temperature to 500°C was compared and analyzed.

[0159] See also Figures 1 to 3 , which is a physical picture of the porous ceramic material obtained in Example 1. Figures 1 to 3 It can be seen that the porous ceramic material of Example 1 has a typical three-dimensional porous structure. After testing, its apparent porosity is 4.36%, the thermal conductivity coefficient is >1.5W / (m·℃), and the flexural strength loss rate is <1.28%. It can be used as a honeycomb ceramic thermal storage body with high thermal shock resistance.

[0160] It can be seen from Tables 1 to 5 that in the porous ceramic materials prepared in Examples 1 to 7, the protective layer loading rate is controlled between 25% and 40%, the apparent porosity is between 3.03% and 10.58%, the thermal conductivity is >1.5W / (m·℃), and the flexural strength loss rate is controlled below 2.46%, which has excellent heat storage performance and thermal shock resistance.

[0161] Taking Example 1 as a reference, no protective layer is formed on the porous ceramic substrate of Comparative Example 1, and its flexural strength loss rate is significantly increased, which is 1.5 to 2.5 times that of Example 1. It can be seen that in the absence of a load protective layer, the porous ceramic substrate works for a long time under high temperature and low temperature frequent alternation conditions, which may cause rupture due to large temperature fluctuations, and may also amplify defects such as microcracks and voids generated during calcination during the preparation process, causing the substrate to shatter and block the air flow channel. Example 1 uses wetting treatment and impregnation treatment to fill, smooth and round the depressions, protrusions, and right angles of the holes in the substrate channels, effectively reducing the phenomenon of thermal stress concentration, so the flexural strength loss rate is greatly reduced.

[0162] Taking Example 1 as a reference, Comparative Example 2 was not wetted before the impregnation treatment, and its protective layer loading rate was only 30% to 60% of that of Example 1, and pores were blocked, and some channels of the substrate had no protective layer inside, resulting in poor coating uniformity. After the comparative example 2 was subjected to a 500°C thermal shock cycle test, the flexural strength loss rate was higher than that before the impregnation due to the large difference in the internal and external materials.

[0163] Taking Example 2 as a reference, magnesium aluminum silicate was not added to the suspension of Comparative Example 3, resulting in an extremely low protective layer loading rate of only 1% to 5%, and a very weak filling and repairing effect on the substrate, resulting in a significant increase in its flexural strength loss rate.

[0164] Taking Example 5 as a reference, no sol was added to the suspension of Comparative Example 4, and the thickness of the protective layer generated on the substrate surface was extremely low, and the protective layer loading rate was significantly reduced. This is because the lack of sol caused the suspension to be unable to form a strong bond with the substrate. During the purge step after impregnation, more than 70% of the suspension in Comparative Example 4 was blown away, while after adding the sol, only 20-30% of the suspension in Example 5 was blown away. In addition, the silica sol / aluminum sol in the sol can also adjust the composition of the suspension to avoid excessive differences in the components of the substrate, thereby preventing the protective layer from falling off.

[0165] Taking Example 6 as a reference, no metal salt was added to the suspension of Comparative Example 5, and its apparent porosity was slightly reduced while the flexural strength loss rate was slightly increased. The reason is that the metal salt molar ratio of Example 6 is Mg:Al:Si = 1:2.1:2.5, while the metal salt molar ratio of Comparative Example 5 is Mg:Al:Si = 1:2:4.2, that is, the suspension only uses magnesium aluminum silicate and silica sol, which easily forms a silicon-rich glass phase and reduces the density of the protective layer.

[0166] Taking Example 7 as a reference, the porous ceramic substrates of Comparative Example 6 and Comparative Example 7 are exactly the same, but the suspension formulas are different. The suspension in Comparative Example 6 contains a higher content of raw materials such as magnesium aluminum silicate and silica sol, so its protective layer loading rate exceeds 40%, making it impossible for the suspension to completely enter the porous ceramic substrate, thereby blocking the pores, resulting in a high apparent porosity and flexural strength loss rate. The suspension in Comparative Example 7 contains less raw materials, resulting in an extremely low protective layer loading rate, and thus having a higher apparent porosity and flexural strength loss rate.

[0167] Table 1. Porous ceramic substrates of Examples 1 to 7

[0168]

[0169] Table 2. Suspensions of Examples 1 to 7

[0170]

[0171] Table 3. Porous ceramic substrates of Comparative Examples 1 to 7

[0172]

[0173] Table 4. Suspensions of Comparative Examples 1 to 7

[0174]

[0175] Table 5. Performance comparison of porous ceramic materials

[0176]

[0177] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0178] The above-described embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of protection of the present application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the scope of protection of the present application. Therefore, the scope of protection of the present application shall be subject to the attached claims.

Claims

1. A porous ceramic material, characterized in that: It comprises a porous ceramic substrate and a protective layer covering the porous ceramic substrate, wherein the mass fraction of the protective layer in the porous ceramic material is 25% to 40%; The raw materials of the porous ceramic matrix include talc, kaolin, a first additive, a second additive, a binder, a pore former, a first dispersant, a lubricant and water; The raw materials of the protective layer include magnesium aluminum silicate, sol, metal salt, a second dispersant and water; Wherein, the first additive comprises one or more of an aluminum source and a silicon source; The second additive includes one or more of mullite whiskers and silicon carbide fibers; The metal salt includes one or more of a magnesium salt and an aluminum salt; In the protective layer, the molar ratio of magnesium element, aluminum element and silicon element is 1:(0.5-5):(0.5-4).

2. The porous ceramic material according to claim 1, characterized in that The porous ceramic matrix comprises the following raw materials in parts by weight: 。 3. The porous ceramic material according to claim 2, characterized in that The protective layer comprises the following raw materials in parts by weight: 。 4. The porous ceramic material according to any one of claims 1 to 3, characterized in that: One or more of the following conditions are met: (1) The aluminum source includes one or more of aluminum oxide, aluminum hydroxide and bauxite; (2) The silicon source includes one or more of silicon powder, quartz sand and yellow sand; (3) In the first additive, the mass ratio of the aluminum source to the silicon source is (0-15):(0-10), and the masses of the aluminum source and the silicon source are not zero at the same time; (4) In the second additive, the mass ratio of the mullite whisker to the silicon carbide fiber is (0-15):(0-10), and the masses of the mullite whisker and the silicon carbide fiber are not zero at the same time.

5. The porous ceramic material according to claim 4, characterized in that One or more of the following conditions are met: (1) The binder includes a cellulose binder; (2) The pore-forming agent includes one or more of an inorganic carbon material and an organic carbon material; (3) the first dispersant and the second dispersant each independently include one or more of oleic acid, sodium oleate, potassium oleate, triethanolamine oleate, polyoxyethylene nonylphenol ether-9 and dodecyltrimethylammonium chloride; (4) The lubricant includes one or more of vegetable oil and mineral oil.

6. The porous ceramic material according to claim 5, characterized in that One or more of the following conditions are met: (1) The magnesium salt includes one or more of magnesium hydroxide, magnesium carbonate, magnesium silicate and magnesium phosphate; (2) The aluminum salt includes one or more of aluminum hydroxide, aluminum dihydrogen phosphate, aluminum silicate and aluminum nitrate; (3) In the metal salt, the mass ratio of the magnesium salt to the aluminum salt is (0-5):(0-10), and the masses of the magnesium salt and the aluminum salt are not zero at the same time; (4) The sol includes one or more of silica sol, aluminum sol, zirconium sol and titanium sol.

7. A method for preparing a porous ceramic material according to any one of claims 1 to 6, characterized in that: The following steps are involved: Mixing talc, kaolin, a first additive, a second additive, a binder, a pore former, a first dispersant, a lubricant and water, and performing mud kneading, aging, mud refining, extrusion molding, first drying and first calcination to prepare a porous ceramic matrix; Wetting the porous ceramic substrate with water vapor to prepare a pretreated substrate; The pre-treated substrate is impregnated with a suspension containing magnesium aluminum silicate, sol, metal salt, a second dispersant and water, and purged, second dried and second calcined to form a protective layer on the pre-treated substrate.

8. The method for preparing a porous ceramic material according to claim 7, characterized in that: The wetting process comprises the following steps: The porous ceramic substrate is wetted by water vapor at a temperature of 110° C. to 150° C. and a pressure of 40 Pa to 380 Pa, and the wetting time is 2 min to 5 min.

9. The method for preparing a porous ceramic material according to claim 7, characterized in that: The first drying method and the second drying method each independently comprise a microwave drying method.

10. The method for preparing a porous ceramic material according to claim 7, characterized in that: The first calcination comprises the following steps: Raise the temperature to 1300℃~1440℃ at a heating rate of 150℃ / h~300℃ / h and keep it at this temperature for 4h~10h.

11. The method for preparing a porous ceramic material according to claim 7, characterized in that: The second calcination comprises the following steps: Raise the temperature to 1250℃~1400℃ at a heating rate of 100℃ / h~200℃ / h and keep it at this temperature for 3h~6h.

12. A honeycomb ceramic heat storage body, characterized in that: The porous ceramic material is made of the porous ceramic material as described in any one of claims 1 to 6, or the porous ceramic material prepared by the method for preparing the porous ceramic material as described in any one of claims 7 to 11.

13. The honeycomb ceramic heat storage body according to claim 12, characterized in that: One or more of the following conditions are met: (1) The heat resistance loss rate of the honeycomb ceramic heat storage body is ≤2.5%; (2) The apparent porosity of the honeycomb ceramic thermal storage body is 1.78% to 12.2%; (3) The thermal conductivity of the honeycomb ceramic thermal storage body is 1.5W / (m·℃)~1.8W / (m·℃).

Citation Information

Patent Citations

  • Ceramic coated automotive heat exchanger components

    CN102575916A

  • Honeycomb ceramic filter and preparation method thereof

    CN102910930A

  • Preparing method of high-temperature-resistant low-apparent-porosity honeycomb ceramic heat accumulator

    CN107879752A

  • Peripheral coating material, a peripheral coating honeycomb structure, and a dust collection filter

    CN110922212A

  • Composite whisker reinforced composite phase change heat storage ball and preparation method thereof

    CN112683095A