Palm polyol ester with good thermal stability and excellent lubricating property as well as preparation method and application of palm polyol ester
By epoxidation, ring opening and esterification reactions of palm oil and palm oleic acid, palm polyol esters with excellent thermal stability and lubricating properties were prepared, which solved the problem of poor thermal stability and oxidative stability of vegetable oil-based lubricants. , realizes a green and environmentally friendly process.
Patent Information
- Application Number
- CN202410923411.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-11-08
AI Technical Summary
Existing vegetable oil-based lubricants have problems such as poor thermal stability, poor oxidation stability and unenvironmental processes, especially in high temperature conditions, and often require the use of organic solvents to participate in the reaction, resulting in pollution and environmental impact.
Palm polyol esters are prepared by epoxidation, ring opening and esterification reactions under the action of an acidic catalyst. The entire process does not require organic solvents, the process is simple, environmentally friendly, and the reaction time is short.
The prepared palm polyol esters have excellent lubricating properties and thermal stability, small viscosity and high viscosity index, can maintain good lubricating properties under high temperature conditions, and have environmentally friendly and pollution-free processes.
Smart Images

Figure CN118908829A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of lubricating oil additives, and in particular to a palm polyol ester with good thermal stability and excellent lubrication performance, and a preparation method and application thereof. Background Art
[0002] The key function of a lubricant is to reduce the resistance to motion between two friction surfaces by forming an oil film, thereby reducing friction and wear. It is estimated that the global consumption of lubricants is nearly 30 million tons per year. Due to the depletion of crude oil reserves and the pollution of mineral oil-based lubricants to the environment, people have begun to turn to vegetable oil-based lubricants. Compared with mineral-based lubricants, vegetable oil-based lubricants are biodegradable, less toxic, and renewable. In addition, the viscosity of vegetable oils changes less with temperature, which ensures that the required lubricating film thickness can be maintained even at higher temperatures. Vegetable oil-based lubricants perform well in applications with a high potential for explosion because they are composed of high molecular weight triglyceride molecules with low volatility and high flash points. Since vegetable oil molecules have a good affinity with metal surfaces, they have good lubricity and excellent corrosion protection properties.
[0003] However, compared with petroleum-based products, renewable products derived from vegetable oils have two major disadvantages: poor oxidative stability and low-temperature operability. Chemical modification of unsaturated double bonds in fatty acids, such as acylation, metathesis, hydroxylation, oxidative cleavage, carboxylation and epoxidation, has been shown to improve the oxidative stability and low-temperature performance of the product. However, the process reaction conditions for preparing vegetable oil-based lubricants in the prior art are relatively harsh, and many side reactions occur. In addition, organic solvents need to be added to participate in the reaction. Since organic solvents are volatile and toxic, they are harmful to the environment and do not meet green benefits. In addition, the vegetable oil-based lubricants in the prior art still have the defect of poor thermal stability, and the reaction takes a long time, pollutants are emitted, and are not green and environmentally friendly. Summary of the invention
[0004] In order to overcome the shortcomings of the prior art, the first object of the present invention is to provide a method for preparing palm polyol ester with good thermal stability and excellent lubrication performance. The preparation reaction process of the preparation method does not require the use of organic solvents, has no side reactions, is simple in process, takes a short reaction time, does not emit pollutants, and is green and environmentally friendly. The prepared palm polyol ester has the advantages of good thermal stability and excellent lubrication performance.
[0005] In order to overcome the deficiencies of the prior art, a second object of the present invention is to provide a palm polyol ester having good thermal stability and excellent lubricity.
[0006] In order to overcome the deficiencies of the prior art, the third object of the present invention is to provide an application of palm polyol ester in a biolubricant.
[0007] In order to achieve the first object of the above invention, the technical solution adopted by the present invention is as follows:
[0008] The present invention provides a method for preparing palm polyol ester with good thermal stability and excellent lubricity, comprising the following steps:
[0009] S1, subjecting palm oil to epoxidation reaction with an acidic catalyst and hydrogen peroxide to obtain epoxidized palm oil;
[0010] S2, subjecting the epoxidized palm oil obtained in step S1 to a ring-opening reaction with palmitoleic acid under the action of a catalyst to obtain palm polyol;
[0011] S3, subjecting the palm polyol obtained in step S2 to an esterification reaction with alcohol under the action of a catalyst to obtain the palm polyol ester.
[0012] The invention discloses a method for preparing a palm polyol ester with good thermal stability and excellent lubricity. The method uses natural products palm oil and palmitoleic acid as raw materials. No organic solvent is required to participate in the reaction during the whole reaction process. First, palm oil is subjected to epoxidation reaction using hydrogen peroxide under the action of an acidic catalyst to generate epoxidized palm oil, thereby expanding the branched chain of the vegetable oil. The whole process meets the requirements of green environmental protection. In addition, the epoxidized palm oil undergoes a ring-opening reaction with palmitoleic acid under the action of a catalyst to obtain palm polyol. The ring-opening reaction expands and extends the carbon chain. The whole reaction is carried out under the conditions of short time consumption and low temperature. There is no tail gas emission at the same time, which meets the benefits of energy saving and environmental protection. In addition, palm polyol undergoes an esterification reaction with alcohol under the action of a catalyst, so that the carbon chain is further extended and expanded, thereby making the prepared palm polyol ester have excellent lubricity while improving the problem of poor thermal stability of palm polyol. Therefore, the preparation reaction process of the preparation method does not require the use of organic solvents, has no side reactions, is simple in process, takes a short reaction time, does not emit pollutants, is green and environmentally friendly, and the prepared palm polyol ester has the advantages of good thermal stability and excellent lubrication performance.
[0013] Among them, after palm oil and hydrogen peroxide undergo epoxidation reaction, epoxidized palm oil is obtained, that is, an epoxy group is formed at the position of the double bond in the palm oil molecule, and the obtained epoxidized palm oil continues to undergo ring-opening reaction with palmitoleic acid, expanding the branch chain and enriching the carbon chain structure of the reactant. In addition, in order to further improve the shortcomings of poor oxidation stability and poor thermal stability of vegetable oil, esterification reaction continues with alcohol to further improve its oxidation stability and thermal stability. In addition, the palm oil and palmitoleic acid used as raw materials of the present invention have the advantages of large output, and compared with other vegetable oils and oleic acid, they also have good oxidation stability, are not easy to deteriorate, and have the advantages of low viscosity and lighter color, and have good lubrication potential. And the palm polyol ester obtained contains more hydroxyl structures, which is conducive to forming a lubricating film at the interface, and thus has good lubrication performance, and the ester structure has good lubrication, and the oxidation stability and thermal stability of the oil ester are improved.
[0014] Furthermore, in step S1, the acidic catalyst is one or a combination of two or more of formic acid, acetic acid or propionic acid; and / or
[0015] In step S1, the molar ratio of hydrogen peroxide to palm oil is (1.1-3.5):1; wherein a slight excess of hydrogen peroxide helps to promote the reaction and improve kinetics, and reduce the occurrence of side reactions; and / or
[0016] The molar ratio of the acid catalyst to palm oil is (0.25-1.5):1; and / or
[0017] The hydrogen peroxide is a hydrogen peroxide aqueous solution with a mass percentage of 30% to 40%.
[0018] Furthermore, in the step S1, the temperature of the epoxidation reaction is 30°C to 105°C, and the reaction time is 3h to 8h.
[0019] Further, in step S2, the molar ratio of palmitoleic acid to epoxidized palm oil is (1.0-3.0):1; and / or
[0020] The amount of the catalyst used accounts for 1% to 5% of the mass of the epoxidized palm oil.
[0021] Furthermore, in step S2, the temperature of the ring-opening reaction is 80°C to 130°C, and the reaction time is 3h to 7h.
[0022] Furthermore, in step S3, the alcohol is at least one of ethylene glycol, ethanol, propanol, propylene glycol or butanediol; and / or
[0023] The catalyst in step S2 and step S3 is one or a combination of two or more of sulfamic acid, p-toluenesulfonic acid and fluoroboric acid; and / or
[0024] The reaction atmosphere of step S2 and step S3 is one of air, nitrogen and argon.
[0025] Further, in step S3, the molar ratio of the palm polyol to the alcohol is 1:(2.0-3.5); and / or
[0026] The amount of the catalyst is 1% to 5% of the mass of the palm polyol; and / or
[0027] The temperature of the esterification reaction is 70° C. to 110° C., and the reaction time is 3 h to 5 h.
[0028] Furthermore, after the esterification reaction in step S3 is completed, the reaction product is washed with a saturated inorganic salt solution, and then extracted with an organic solvent, and allowed to stand for stratification to separate the aqueous phase and the organic phase, and the organic phase obtained after removing the organic solvent is the palm polyol ester; and / or
[0029] The saturated inorganic salt solution is one or a combination of two or more of a sodium carbonate solution, a sodium bicarbonate solution and a sodium chloride solution; and / or
[0030] The organic solvent is one or a combination of two or more of ethyl acetate, dichloromethane and n-hexane.
[0031] The purpose of washing is to remove other substances mixed in the oil and facilitate the separation of the organic phase and the aqueous phase. The extraction is to enrich the oil as much as possible in the organic phase, thereby improving the efficiency of separation of the oil layer and the aqueous layer. The separated organic phase is subjected to rotary evaporation to remove the organic solvent, thereby obtaining palm polyol esters.
[0032] In order to achieve the second purpose of the above invention, the technical solution adopted by the present invention is as follows:
[0033] The invention provides a palm polyol ester with good thermal stability and excellent lubricity, which is prepared by the above-mentioned method for preparing the palm polyol ester with good thermal stability and excellent lubricity.
[0034] The starting temperature of thermal decomposition and oxidation of the prepared palm polyol ester in air atmosphere is 297.5°C, the viscosity index is 175-189, and the kinematic viscosity is 29.41-38.13 mm 2 / S, maximum no-seizure load P in four-ball friction test B ≤88kg, maximum sintering load P D≤620kg, the friction coefficient curve is smooth and stable. Therefore, the prepared palm polyol ester has the characteristics of good thermal stability, low viscosity, high viscosity index and excellent lubrication performance.
[0035] In order to achieve the third purpose of the above invention, the technical solution adopted by the present invention is as follows:
[0036] The present invention provides a plant oil-based lubricant, and uses the palm polyol ester prepared by the above-mentioned method for preparing the palm polyol ester with good thermal stability and excellent lubrication performance in the lubricant;
[0037] The palm polyol ester is used alone as the vegetable oil-based lubricant; or, the palm polyol ester is added to a base oil as a lubricant additive to form the vegetable oil-based lubricant.
[0038] Among them, since the vegetable oil-based lubricant of the present invention includes the palm polyol ester with good thermal stability and excellent lubrication performance prepared by the present invention, the vegetable oil-based lubricant has the advantages of good oxidation and thermal decomposition stability and excellent lubrication performance.
[0039] In addition, the plant oil-based lubricant of the present invention has a maximum non-seizure load PB≤88kg and a maximum sintering load PD≤620kg in a four-ball friction test, has a strong load-bearing capacity, and a smooth and stable friction coefficient curve, and is a biolubricant with excellent lubrication performance.
[0040] Compared with the prior art, the present invention has the following beneficial effects:
[0041] (1) The method for preparing a palm polyol ester with good thermal stability and excellent lubricity of the present invention uses natural products palm oil and palmitoleic acid as raw materials. No organic solvent is required to participate in the reaction during the entire reaction process. First, palm oil is subjected to epoxidation reaction using hydrogen peroxide under the action of an acidic catalyst to generate epoxidized palm oil, thereby expanding the branched chain of the vegetable oil. The entire process meets the requirements of green environmental protection. In addition, the epoxidized palm oil undergoes a ring-opening reaction with palmitoleic acid under the action of a catalyst to obtain palm polyols. The ring-opening reaction expands and extends the carbon chain, and the entire reaction is carried out under the conditions of short time consumption and low temperature, and there is no tail gas emission, which meets the benefits of energy saving and environmental protection. In addition, palm polyols undergo an esterification reaction with alcohol under the action of a catalyst, so that the carbon chain is further extended and expanded, so that the palm polyol ester obtained has excellent lubricity while improving the problem of poor thermal stability of palm polyols. Therefore, the preparation reaction process of the preparation method does not require the use of organic solvents, has no side reactions, is simple in process, takes a short reaction time, does not emit pollutants, is green and environmentally friendly, and the prepared palm polyol ester has the advantages of good thermal stability and excellent lubrication properties.
[0042] (2) After the palm oil of the present invention undergoes epoxidation reaction with hydrogen peroxide, epoxidized palm oil is obtained, that is, an epoxy group is formed at the position of the double bond in the palm oil molecule. After the obtained epoxidized palm oil continues to undergo a ring-opening reaction with palmitoleic acid, the branched chain is expanded and the carbon chain structure of the reactant is enriched. In addition, in order to further improve the shortcomings of poor oxidation stability and poor thermal stability of vegetable oils, an esterification reaction continues with alcohol to further improve its oxidation stability and thermal stability. In addition, the palm oil and palmitoleic acid used as raw materials in the present invention have the advantages of large yield. Compared with other vegetable oils and oleic acid, they also have the advantages of good oxidation stability, not easy to deteriorate, low viscosity, and lighter color, and have good lubrication potential. In addition, the palm polyol ester obtained contains more hydroxyl structures, which is conducive to forming a lubricating film at the interface, and thus has good lubrication performance. At the same time, the ester structure has good lubrication and improves the oxidation stability and thermal stability of the oil ester.
[0043] (3) The palm polyol ester of the present invention has good thermal stability and excellent lubricity, and the starting temperature of thermal decomposition and oxidation in air atmosphere is 297.5°C, the viscosity index is 175-189, and the kinematic viscosity is 29.41-38.13 mm 2 / S, maximum no-seizure load P in four-ball friction test B ≤88kg, maximum sintering load P D ≤620kg, the friction coefficient curve is smooth and stable. Therefore, the prepared palm polyol ester has the characteristics of good thermal stability, low viscosity, high viscosity index and excellent lubrication performance.
[0044] (4) A plant oil-based lubricant of the present invention comprises the palm polyol ester with good thermal stability and excellent lubrication performance prepared by the present invention. Therefore, the plant oil-based lubricant has the advantages of good oxidation and thermal decomposition stability and excellent lubrication performance. In addition, in the four-ball friction test, the plant oil-based lubricant has a maximum non-seizure load PB≤88kg and a maximum sintering load PD≤620kg, has a strong load-bearing capacity, and a smooth and stable friction coefficient curve, and is a biolubricant with excellent lubrication performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0046] Figure 1It is the infrared spectra of the raw material palm oil of the present invention and the epoxidized palm oil and palm polyol ester prepared in Example 1.
[0047] Figure 2 This is the hydrogen nuclear magnetic resonance spectrum of the epoxidized palm oil prepared in Example 1 of the present invention.
[0048] Figure 3 It is the hydrogen nuclear magnetic resonance spectrum of the palm polyol ester prepared in Example 1 of the present invention.
[0049] Figure 4 The friction coefficient-time curves are obtained by performing four-ball tribology experiments on the palm polyol ester prepared in Example 1 of the present invention and the raw material palm oil.
[0050] Figure 5 The palm polyol ester prepared in Example 1 of the present invention and the raw material palm oil were subjected to four-ball tribology experiments, and the wear spot morphology of the wear area of the steel ball was observed using an electron microscope. In the figure, a, b, and c are the surface morphologies of the wear spots under the lubrication of palm polyol ester; d, e, and f are the surface morphologies of the wear spots under the lubrication of palm oil.
[0051] Figure 6 It is a thermal decomposition weight loss curve of raw material palm oil, intermediate product epoxidized palm oil and palm polyol of Example 1, and palm polyol ester prepared in Example 1 and Example 2. DETAILED DESCRIPTION
[0052] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0053] The terms used in the embodiments of the present invention are only for the purpose of describing specific embodiments, and are not intended to limit the present invention. In the present invention, the singular forms "a", "said" and "the" used in the embodiments and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.
[0054] In an embodiment of the present invention, a method for preparing palm polyol ester with good thermal stability and excellent lubricity comprises the following steps:
[0055] S1, subjecting palm oil to epoxidation reaction with an acidic catalyst and hydrogen peroxide to obtain epoxidized palm oil;
[0056] S2, subjecting the epoxidized palm oil obtained in step S1 to a ring-opening reaction with palmitoleic acid under the action of a catalyst to obtain palm polyol;
[0057] S3, subjecting the palm polyol obtained in step S2 to an esterification reaction with alcohol under the action of a catalyst to obtain the palm polyol ester.
[0058] A method for preparing a palm polyol ester with good thermal stability and excellent lubricity in the embodiment is to use natural products palm oil and palmitoleic acid as raw materials, and no organic solvent is required to participate in the reaction during the whole reaction process. First, palm oil is subjected to epoxidation reaction using hydrogen peroxide under the action of an acidic catalyst to generate epoxidized palm oil, thereby expanding the branched chain of vegetable oil, and the whole process meets the requirements of green environmental protection. In addition, epoxidized palm oil undergoes a ring-opening reaction with palmitoleic acid under the action of a catalyst to obtain palm polyols, and the ring-opening reaction expands and extends the carbon chain, and the whole reaction is carried out under the conditions of short time consumption and low temperature, and there is no tail gas emission at the same time, which meets the benefits of energy saving and environmental protection. In addition, palm polyols undergo an esterification reaction with alcohol under the action of a catalyst, so that the carbon chain is further extended and expanded, so that the obtained palm polyol ester has excellent lubricity while improving the problem of poor thermal stability of palm polyols. Therefore, the preparation reaction process of the preparation method does not require the use of organic solvents, has no side reactions, is simple in process, takes a short reaction time, does not emit pollutants, is green and environmentally friendly, and the prepared palm polyol ester has the advantages of good thermal stability and excellent lubrication performance.
[0059] Among them, after palm oil and hydrogen peroxide undergo epoxidation reaction, epoxidized palm oil is obtained, that is, an epoxy group is formed at the position of the double bond in the palm oil molecule, and the obtained epoxidized palm oil continues to undergo ring-opening reaction with palmitoleic acid, expanding the branch chain and enriching the carbon chain structure of the reactant. In addition, in order to further improve the shortcomings of poor oxidation stability and poor thermal stability of vegetable oil, esterification reaction continues with alcohol to further improve its oxidation stability and thermal stability. In addition, the palm oil and palmitoleic acid used as raw materials of the present invention have the advantages of large output, and compared with other vegetable oils and oleic acid, they also have good oxidation stability, are not easy to deteriorate, and have the advantages of low viscosity and lighter color, and have good lubrication potential. And the palm polyol ester obtained contains more hydroxyl structures, which is conducive to forming a lubricating film at the interface, and thus has good lubrication performance, and the ester structure has good lubrication, and the oxidation stability and thermal stability of the oil ester are improved.
[0060] In some embodiments, in step S1, the acidic catalyst is one or a combination of two or more of formic acid, acetic acid or propionic acid; and / or
[0061] In step S1, the molar ratio of hydrogen peroxide to palm oil is (1.1-3.5):1; wherein a slight excess of hydrogen peroxide helps to promote the reaction and improve kinetics, and reduce the occurrence of side reactions; and / or
[0062] The molar ratio of the acid catalyst to palm oil is (0.25-1.5):1; and / or
[0063] The hydrogen peroxide is a hydrogen peroxide aqueous solution with a mass percentage of 30% to 40%.
[0064] In some embodiments, in step S1, the temperature of the epoxidation reaction is 30°C to 105°C, and the reaction time is 3h to 8h.
[0065] In some embodiments, in step S2, the molar ratio of palmitoleic acid to epoxidized palm oil is (1.0-3.0):1; and / or
[0066] The amount of the catalyst used accounts for 1% to 5% of the mass of the epoxidized palm oil.
[0067] In some embodiments, in step S2, the temperature of the ring-opening reaction is 80° C. to 130° C., and the reaction time is 3 h to 7 h.
[0068] In some embodiments, in step S3, the alcohol is at least one of ethylene glycol, ethanol, propanol, propylene glycol or butanediol; and / or
[0069] The catalyst in step S2 and step S3 is one or a combination of two or more of sulfamic acid, p-toluenesulfonic acid and fluoroboric acid; and / or
[0070] The reaction atmosphere of step S2 and step S3 is one of air, nitrogen and argon.
[0071] In some embodiments, in step S3, the molar ratio of palm polyol to alcohol is 1:(2.0-3.5); and / or
[0072] The amount of the catalyst is 1% to 5% of the mass of the palm polyol; and / or
[0073] The temperature of the esterification reaction is 70° C. to 110° C., and the reaction time is 3 h to 5 h.
[0074] In some embodiments, after the esterification reaction in step S3 is completed, the reaction product is washed with a saturated inorganic salt solution, and then extracted with an organic solvent, and the layers are allowed to stand to separate the aqueous phase and the organic phase, and the organic phase obtained after removing the organic solvent is the palm polyol ester; and / or
[0075] The saturated inorganic salt solution is one or a combination of two or more of a sodium carbonate solution, a sodium bicarbonate solution and a sodium chloride solution; and / or
[0076] The organic solvent is one or a combination of two or more of ethyl acetate, dichloromethane and n-hexane.
[0077] The purpose of washing is to remove other substances mixed in the oil and facilitate the separation of the organic phase and the aqueous phase. The extraction is to enrich the oil as much as possible in the organic phase, thereby improving the efficiency of separation of the oil layer and the aqueous layer. The separated organic phase is subjected to rotary evaporation to remove the organic solvent, thereby obtaining palm polyol esters.
[0078] In an embodiment of the present invention, a palm polyol ester with good thermal stability and excellent lubricity is prepared by the above-mentioned method for preparing a palm polyol ester with good thermal stability and excellent lubricity.
[0079] The starting temperature of thermal decomposition and oxidation of the prepared palm polyol ester in air atmosphere is 297.5°C, the viscosity index is 175-189, and the kinematic viscosity is 29.41-38.13 mm 2 / S, maximum no-seizure load P in four-ball friction test B ≤88kg, maximum sintering load P D ≤620kg, the friction coefficient curve is smooth and stable. Therefore, the prepared palm polyol ester has the characteristics of good thermal stability, low viscosity, high viscosity index and excellent lubrication performance.
[0080] In an embodiment of the present invention, a plant oil-based lubricant, use of the palm polyol ester prepared by the above-mentioned method for preparing a palm polyol ester with good thermal stability and excellent lubrication performance in the lubricant;
[0081] The palm polyol ester is used alone as the vegetable oil-based lubricant; or, the palm polyol ester is added to a base oil as a lubricant additive to form the vegetable oil-based lubricant.
[0082] Among them, since the vegetable oil-based lubricant of the present invention includes the palm polyol ester with good thermal stability and excellent lubrication performance prepared by the present invention, the vegetable oil-based lubricant has the advantages of good oxidation and thermal decomposition stability and excellent lubrication performance.
[0083] In addition, the plant oil-based lubricant of the present invention has a maximum non-seizure load PB≤88kg and a maximum sintering load PD≤620kg in a four-ball friction test, has a strong load-bearing capacity, and a smooth and stable friction coefficient curve, and is a biolubricant with excellent lubrication performance.
[0084] The following describes the invention in conjunction with specific embodiments.
[0085] Example 1
[0086] A method for preparing palm polyol ester with good thermal stability and excellent lubricity comprises the following steps:
[0087] S1. Preparation of epoxidized palm oil: 138.53 g of palm oil was stirred and heated in a constant temperature water bath. After the temperature was raised to 72°C, 35.40 mL of acidic catalyst propionic acid was added, preheated for a period of time, 76.32 mL of hydrogen peroxide solution was slowly and dropwise added, and the reaction was carried out at a temperature of 72°C for 7 hours. After the reaction was completed, it was cooled to room temperature, washed with saturated sodium chloride solution 2-3 times, extracted with solvent ethyl acetate, allowed to stand for a period of time, the upper organic phase was taken, vacuum rotary evaporation was performed, the organic solvent was removed, and the residual catalyst was removed by centrifugation to obtain a light yellow clear oily liquid, which was epoxidized palm oil; in this embodiment, the mass percentage concentration of the hydrogen peroxide solution was 35%;
[0088] S2, preparation of palm polyol: 107.15g of epoxidized palm oil obtained in S1 was stirred and heated in a constant temperature water bath, heated to 80°C in an air atmosphere, 1.00g of catalyst p-toluenesulfonic acid was added, then heated to 110°C, 45.50g of palmitoleic acid was added, and the reaction was carried out for 4h. After the reaction was completed, it was washed with a saturated sodium chloride solution for 2-3 times, extracted with a solvent ethyl acetate, allowed to stand for a period of time, the upper organic phase was taken, vacuum rotary evaporation was carried out to remove the organic solvent, and a yellow clear oily liquid was obtained, which was palm polyol;
[0089] S3, preparation of palm polyol ester: take 100.205g of palm polyol obtained in S2 and heat it to 80°C, add 3.6mL of catalyst fluoroboric acid, add 54.1mL of ethylene glycol dropwise in an air atmosphere, react for 4h, wash with saturated sodium chloride solution 2-3 times after the reaction, extract with solvent ethyl acetate, let stand for a while, take the upper organic phase, vacuum evaporate and remove the organic solvent to obtain a yellow oily liquid with ester aroma, which is palm polyol ester.
[0090] Example 2
[0091] A method for preparing palm polyol ester with good thermal stability and excellent lubricity comprises the following steps:
[0092] S1. Preparation of epoxidized palm oil: 102.57g of palm oil was stirred and heated in a constant temperature water bath. After the temperature was raised to 72°C, 33.54mL of acidic catalyst propionic acid was added, preheated for a period of time, 73.12mL of hydrogen peroxide solution was slowly and dropwise added, and the reaction was carried out at a temperature of 72°C for 7h. After the reaction was completed, it was cooled to room temperature, washed with saturated sodium chloride solution 2-3 times, extracted with solvent ethyl acetate, allowed to stand for a period of time, the upper organic phase was taken, vacuum rotary evaporation was performed, the organic solvent was removed, and the residual catalyst was removed by centrifugation to obtain a light yellow clear oily liquid, which was epoxidized palm oil; in this embodiment, the mass percentage concentration of the hydrogen peroxide solution was 35%;
[0093] S2, preparation of palm polyol: 121.04g of epoxidized palm oil obtained in S1 was stirred and heated in a constant temperature water bath, heated to 80°C in an air atmosphere, 1.22g of aminosulfonic acid as a catalyst was added, then heated to 110°C, 57.16g of palmitoleic acid was added, and the reaction was carried out for 4h. After the reaction, the mixture was washed 2-3 times with a saturated sodium chloride solution, extracted with ethyl acetate as a solvent, allowed to stand for a period of time, the upper organic phase was taken, vacuum rotary evaporation was performed to remove the organic solvent, and a yellow clear oily liquid was obtained, which was palm polyol;
[0094] S3, preparation of palm polyol ester: take 100.205g of palm polyol obtained in S2, heat it to 80°C, add 2.938g of aminosulfonic acid as a catalyst, add 54.1mL of ethylene glycol dropwise in an air atmosphere, react for 4h, wash with saturated sodium chloride solution 2-3 times after the reaction, extract with solvent ethyl acetate, let stand for a while, take the upper organic phase, vacuum evaporate and remove the organic solvent to obtain a yellow oily liquid with ester aroma, which is palm polyol ester.
[0095] Example 3
[0096] A method for preparing palm polyol ester with good thermal stability and excellent lubricity comprises the following steps:
[0097] S1. Palm oil is subjected to epoxidation reaction with an acidic catalyst, formic acid and hydrogen peroxide at 30° C. for 8 hours to obtain epoxidized palm oil. In this embodiment, the molar ratio of hydrogen peroxide to palm oil is 2:1; the molar ratio of the acidic catalyst, formic acid, to palm oil is 1:1; and the hydrogen peroxide is a 30% by mass aqueous solution of hydrogen peroxide.
[0098] S2, the epoxidized palm oil obtained in step S1 and palmitoleic acid are subjected to a ring-opening reaction at 100° C. for 4 hours under the action of a catalyst, aminosulfonic acid, to obtain palm polyol; in this embodiment, the molar ratio of palmitoleic acid to epoxidized palm oil is 2.0:1; the amount of the catalyst is 3% of the mass of the epoxidized palm oil; the reaction atmosphere of this step is air;
[0099] S3, the palm polyol obtained in step S2 and propanol are subjected to esterification reaction at 90° C. for 4 hours under the action of aminosulfonic acid as a catalyst, so as to obtain the palm polyol ester. In this embodiment, the molar ratio of palm polyol to alcohol is 1:3.0; the amount of the catalyst used accounts for 3% of the mass of the palm polyol.
[0100] After the esterification reaction in step S3 is completed, the reaction product is washed with a saturated sodium carbonate solution, and then extracted with an organic solvent ethyl acetate. The mixture is allowed to stand for stratification to separate the aqueous phase and the organic phase. The organic phase obtained after removing the organic solvent is palm polyol ester.
[0101] Example 4
[0102] A method for preparing palm polyol ester with good thermal stability and excellent lubricity comprises the following steps:
[0103] S1. Palm oil is subjected to epoxidation reaction with an acidic catalyst, acetic acid, and hydrogen peroxide at 105° C. for 3 hours to obtain epoxidized palm oil. In this embodiment, the molar ratio of hydrogen peroxide to palm oil is 1.1:1; the molar ratio of the acidic catalyst, acetic acid, to palm oil is 0.25:1; and the hydrogen peroxide is a 40% by mass aqueous solution of hydrogen peroxide.
[0104] S2, the epoxidized palm oil obtained in step S1 and palmitoleic acid are subjected to a ring-opening reaction at 80° C. for 7 hours under the action of a catalyst of p-toluenesulfonic acid to obtain palm polyol; in this embodiment, the molar ratio of palmitoleic acid to epoxidized palm oil is 1:1; the amount of the catalyst used accounts for 1% of the mass of the epoxidized palm oil; the reaction atmosphere of this step is nitrogen;
[0105] S3, the palm polyol obtained in step S2 and ethanol are subjected to esterification reaction at 70° C. for 5 hours under the action of p-toluenesulfonic acid as a catalyst, so as to obtain the palm polyol ester. In this embodiment, the molar ratio of palm polyol to alcohol is 1:2.0; the amount of the catalyst used accounts for 1% of the mass of the palm polyol.
[0106] After the esterification reaction in step S3 is completed, the reaction product is washed with a saturated sodium bicarbonate solution, and then extracted with an organic solvent, dichloromethane, and allowed to stand for stratification to separate the aqueous phase and the organic phase. The organic phase obtained after removing the organic solvent is palm polyol ester.
[0107] Example 5
[0108] A method for preparing palm polyol ester with good thermal stability and excellent lubricity comprises the following steps:
[0109] S1. Carry out epoxidation reaction of palm oil with acidic catalyst formic acid and hydrogen peroxide at 50° C. for 7 hours to obtain epoxidized palm oil. In this embodiment, the molar ratio of hydrogen peroxide to palm oil is 1.25:1; the molar ratio of acidic catalyst formic acid to palm oil is 0.75:1; and the hydrogen peroxide is a 32% by mass aqueous solution of hydrogen peroxide.
[0110] S2, the epoxidized palm oil obtained in step S1 and palmitoleic acid are subjected to a ring-opening reaction at 130° C. for 3 hours under the action of a catalyst, fluoroboric acid, to obtain palm polyol; in this embodiment, the molar ratio of palmitoleic acid to epoxidized palm oil is 3:1; the amount of the catalyst used accounts for 5% of the mass of the epoxidized palm oil; the reaction atmosphere of this step is argon;
[0111] S3, the palm polyol obtained in step S2 is subjected to an esterification reaction with a combination of propylene glycol and butanediol at 110° C. for 3 hours under the action of a catalyst, fluoroboric acid, to obtain the palm polyol ester. In this embodiment, the molar ratio of palm polyol to alcohol is 1:3.5; the amount of the catalyst used accounts for 5% of the mass of the palm polyol.
[0112] After the esterification reaction in step S3 is completed, the reaction product is washed with a saturated sodium chloride solution, and then extracted with an organic solvent, n-hexane, and allowed to stand for stratification to separate the aqueous phase and the organic phase. The organic phase obtained after removing the organic solvent is palm polyol ester.
[0113] Example 6
[0114] A vegetable oil-based lubricant, comprising the use of a palm polyol ester prepared by any one of the methods for preparing a palm polyol ester having good thermal stability and excellent lubricity in embodiments 1 to 5 in a lubricant;
[0115] The prepared palm polyol ester is used alone as a vegetable oil-based lubricant.
[0116] Example 7
[0117] A vegetable oil-based lubricant, comprising the use of a palm polyol ester prepared by any one of the methods for preparing a palm polyol ester having good thermal stability and excellent lubricity in embodiments 1 to 5 in a lubricant;
[0118] The prepared palm polyol ester is added into base oil as a lubricant additive to form a vegetable oil-based lubricant.
[0119] Experimental testing
[0120] (I) Structural morphology characterization
[0121] (1) Structural characterization by infrared spectroscopy
[0122] The raw material palm oil and the epoxidized palm oil and palm polyol ester prepared in Example 1 were characterized by infrared spectroscopy. Figure 1 As shown. Figure 1 The chemical changes from raw palm oil to epoxidized palm oil can be clearly seen in the infrared spectrum of the raw palm oil. In the original state, the double bond (C=C) of the raw palm oil is at 3000cm -1 A small peak was detected at 2960 cm-1. -1 and 2860cm -1 . At 1742cm -1The characteristic ester carbonyl group (C=O) appeared at 1170-1240 cm -1 Within range. 722cm -1 The peak at 825cm corresponds to the presence of fatty chains. After the epoxidation reaction, the double bonds of the raw palm oil disappear. -1 A new peak appeared at 820-840cm, confirming the formation of epoxy group (COC), that is, the generation of epoxidized palm oil. -1 The epoxy bond was detected within the bandwidth of 825.10 cm-1. -1 There is a peak of epoxy group (COC) at 3000cm. After the reaction, the palm polyol generated disappears. -1 A new double bond peak appeared near 1270 cm -1 A relatively weak functional group secondary alcohol (-OH) peak appeared nearby, proving that a ring-opening reaction had occurred and a new group had been introduced.
[0123] (2) Structural characterization by H NMR spectroscopy
[0124] The epoxidized palm oil prepared in Example 1 was characterized by hydrogen nuclear magnetic resonance spectroscopy. Figure 2 As shown. Figure 2 It can be seen that the epoxidized palm oil obtained by epoxidizing the raw material palm oil is dissolved in DMSO-d6, and the recorded 1 HNMR (400MHz) spectrum provides product distribution. Raw palm oil is epoxidized, and the possible composition of the product is shown in the structures ①, ②, and ③ in the figure. Among them, the epoxidation process can be proved by the disappearance of olefin protons near 5.3ppm (C=CH) and methylene protons at 1.9-2.0ppm methylene (-CH2). It can also be seen from the spectrum that there is no peak near 5.3ppm, and the signal near 1.9ppm is weak, indicating that the epoxidation reaction is in progress; the number of impurity peaks is small, indicating that the epoxidized palm oil obtained has few impurities; the chemical shift δ is near 0.9ppm and 1.2ppm, which are the chemical shifts of methyl and methylene protons respectively; δ is near 1.9ppm, which is the proton on the methyl connected to the double bond carbon atom, the peak integral is small, and the signal is weak, which proves that the content of raw palm oil is low and the raw material conversion rate is high; the signal peak of the epoxy group is near 3.3ppm-3.4ppm, and there are also absorption peaks of methyl and methylene connected to oxygen atoms on the carbon chain nearby, so the peak integral at this place is the largest.
[0125] The palm polyol ester prepared in Example 1 was characterized by hydrogen nuclear magnetic resonance spectroscopy. Figure 3 As shown. Figure 3 It can be seen that the palm polyol esters prepared by ring-opening reaction of epoxidized palm oil are dissolved in DMSO-d6 and the recorded 1 HNMR (400MHz) spectrum provides product distribution. Palmitoleic acid and epoxidized palm oil undergo ring-opening reaction, and the possible composition of the product is shown in the structure of ①, ②, ③, ④, and ⑤ in the figure. Among them, the terminal methyl signal is obtained at δ of 0.83ppm-0.94ppm. The peak near δ of 1.2ppm belongs to the internal (-CH2-) group present in the fatty acid chain. The proton of the methylene group next to the carbonyl functional group corresponds to δ of 2.32ppm-2.34ppm. The detection of epoxy groups at chemical shifts δ of 0.9ppm, 1.2ppm, and 1.5ppm are chemical shifts of protons connected to methyl, methylene, and methyne, respectively. Affected by the adjacent hydrogen atoms on the carbon chain, more split peaks appear, and the corresponding peak area is also the largest; at δ of 2.0ppm-2.4ppm, it belongs to the protons on the methyl group connected to the double bond carbon atom. Also affected by the adjacent hydrogen atoms on the carbon chain, more split peaks appear; at δ of 2.50ppm, it is the solvent peak of deuterated dimethyl sulfoxide (DMSO-d); at δ of 3.3ppm, it is the absorption peak of the methyl and methylene connected to the oxygen atom on the carbon chain; at δ of 3.9ppm, it is the proton peak on the carbon atom connected to the ester group; at δ of 5.3ppm-5.4ppm, it is the chemical shift of the proton on the double bond carbon atom, proving that the double bond still exists and a small amount of oleic acid has not reacted. At the same time, the signal detected at δ of 5.3ppm is sp 2 For hybrid carbon-carbon double bonds, as the unsaturation is converted into epoxy bonds, the double bond peak disappears, and due to the addition of oleic acid to the structure of palm polyol, the unsaturated peak appears again in the spectrum.
[0126] (II) Tribological performance test
[0127] The palm polyol ester prepared in Example 1 and the raw material palm oil were respectively subjected to tribological performance tests and comparisons, specifically, the characterization of the friction coefficient curve and the characterization of the wear spot morphology under an electron microscope were respectively carried out.
[0128] (1) Characterization of friction coefficient curve
[0129] The palm polyol ester prepared in Example 1 and the raw material palm oil were subjected to four-ball tribology tests under the experimental conditions of a rotation speed of 1200 r / min and a load of 40 kg, and the friction coefficient-time curves were obtained as shown in FIG. Figure 4 The friction experiment can be divided into two stages: the first stage is the running-in stage, and the initial friction curve is unstable and oscillates greatly; the second stage is after the running-in stage, and the friction coefficient curve tends to be stable. During the friction process, the friction coefficient changes slightly with the change of contact area.
[0130] Depend on Figure 4 It can be seen that the palm oil curve fluctuates up and down in the first stage, and it does not stabilize until after 400s. However, the palm polyol ester prepared in Example 1 is always in a stable state. It can be seen that the palm polyol ester obtained by the epoxidation reaction, ring-opening reaction and esterification reaction of palm oil can greatly improve its tribological properties.
[0131] In addition, the palm polyol ester prepared in Example 1 and the raw material palm oil were used as lubricants to carry out four-ball test lubrication load capacity determination according to the method of GB / T3142. The tribological performance test results are shown in Table 1.
[0132] Table 1 Tribological properties test results of palm polyol ester and raw material palm oil
[0133]
[0134] From the test results in Table 1, it can be seen that the maximum non-seizure load (P B ) and the maximum sintering load (P D ) are better than raw palm oil.
[0135] (2) Characterization of wear spot morphology under electron microscope
[0136] The palm polyol ester prepared in Example 1 and the raw material palm oil were subjected to four-ball tribology test under the experimental conditions of a rotation speed of 1200 r / min and a load of 40 kg, and then the wear spot morphology of the wear area of the steel ball was observed by electron microscopy. Figure 5 .
[0137] in, Figure 5 Figures a, b, and c show the surface morphology of the wear spots under lubrication of palm polyol ester. Figure 5 Figures d, e, and f show the surface morphologies of wear spots under palm oil lubrication.
[0138] Depend on Figure 5 As can be seen from Figures a, b, and c, the surface of the wear spot under the lubrication of palm polyol ester is smooth and flat, without deep scratches and abrasions, the wear mark furrows are shallow and smooth, and there are no uneven flaking pits and shadows. This proves that the palm polyol ester prepared by the present invention forms an effective lubricating film, reduces friction, and has a good lubrication effect.
[0139] Depend on Figure 5It can be seen from Figures d, e, and f that there are many unevenly sized peeling pits and shadows on the surface of the wear spot under the lubrication of raw palm oil. Friction debris of particles is produced after friction, and a granular morphology appears. The abrasions are deep, the wear mark grooves are deep, and they are not smooth enough, indicating that it is difficult to form an effective lubricating film under the lubrication of raw palm oil, resulting in poor anti-wear and wear-reducing performance.
[0140] (II) Various performance tests
[0141] The raw material palm oil, the epoxidized palm oil, palm polyol and palm polyol ester respectively prepared in Example 1, and the palm polyol ester prepared in Example 2 were tested for kinematic viscosity, viscosity index, flash point, acid value, hydroxyl value and thermal decomposition starting temperature. Among them, the kinematic viscosity adopts the test method of GB / T265, the viscosity index adopts the test method of GB / T2541, the flash point adopts the method of GB / T3536, the acid value and hydroxyl value adopt the method of GB / T264, and the thermal decomposition starting temperature adopts the method of TG / DTA test. The test results of the above items are shown in Table 2.
[0142] Table 2 Performance parameter test results of raw material palm oil and each product obtained in Example 1-2
[0143]
[0144] As can be seen from the test results of Table 2, the palm polyol ester obtained by epoxidation reaction, ring-opening reaction and esterification reaction in Example 1 and Example 2 of the present invention is an orange transparent clear liquid. The obtained palm polyol ester has good thermal stability and excellent lubrication performance. Compared with the raw material palm oil, the epoxidized palm oil and palm polyol of the intermediate product of Example 1, the viscosity index, flash point, hydroxyl value and thermal decomposition temperature of the palm polyol ester are increased. Since the palm polyol ester obtained by the present invention has a greatly improved hydroxyl value and low viscosity, it is proved that the number of functional groups contained in the palm polyol ester increases, which helps to form chemical bonds with the metal surface during the friction lubrication process, promote the generation of lubricating film, and play a role in lubrication buffering and protection. In addition, the thermal decomposition start temperature of the palm polyol ester obtained in Example 1 is compared with the epoxidized palm oil and palm polyol of the intermediate product of Example 1. While the number of functional groups increases, the thermal stability is improved.
[0145] In addition, it can be seen from the test results in Table 2 that compared with the palm polyol esters prepared in Example 1 and Example 2, the kinematic viscosity, viscosity index, flash point, acid value, hydroxyl value, and thermal decomposition starting temperature of the palm polyol ester of Example 1 are better than those of the palm polyol ester of Example 2, indicating that in the ring-opening reaction of step S2, the catalyst selection of p-toluenesulfonic acid is better than aminosulfonic acid. Therefore, the difference in catalysts will affect the composition of the product, and then affect the performance parameters of the product.
[0146] The thermal decomposition weight loss curves of the raw material palm oil, the intermediate product epoxidized palm oil and palm polyol of Example 1, and the palm polyol esters prepared in Examples 1 and 2 are shown in FIG. Figure 6 .
[0147] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application.
Claims
1. A method for preparing palm polyol ester with good thermal stability and excellent lubricity, characterized in that: The following steps are involved: S1, subjecting palm oil to epoxidation reaction with an acidic catalyst and hydrogen peroxide to obtain epoxidized palm oil; S2, subjecting the epoxidized palm oil obtained in step S1 to a ring-opening reaction with palmitoleic acid under the action of a catalyst to obtain palm polyol; S3, subjecting the palm polyol obtained in step S2 to an esterification reaction with alcohol under the action of a catalyst to obtain the palm polyol ester.
2. The method for preparing a palm polyol ester having good thermal stability and excellent lubricity as claimed in claim 1, characterized in that: In step S1, the acidic catalyst is one or a combination of two or more of formic acid, acetic acid or propionic acid; and / or In the step S1, the molar ratio of hydrogen peroxide to palm oil is (1.1-3.5):1; and / or The molar ratio of the acid catalyst to palm oil is (0.25-1.5):1; and / or The hydrogen peroxide is a hydrogen peroxide aqueous solution with a mass percentage of 30% to 40%.
3. The method for preparing a palm polyol ester having good thermal stability and excellent lubricity as claimed in claim 1, characterized in that: In the step S1, the temperature of the epoxidation reaction is 30° C. to 105° C., and the reaction time is 3 h to 8 h.
4. The method for preparing a palm polyol ester having good thermal stability and excellent lubricity as claimed in claim 1, characterized in that: In the step S2, the molar ratio of palmitoleic acid to epoxidized palm oil is (1.0-3.0):1; and / or The amount of the catalyst used accounts for 1% to 5% of the mass of the epoxidized palm oil.
5. The method for preparing a palm polyol ester having good thermal stability and excellent lubricity as claimed in claim 1, characterized in that: In the step S2, the temperature of the ring-opening reaction is 80° C. to 130° C., and the reaction time is 3 h to 7 h.
6. The method for preparing a palm polyol ester having good thermal stability and excellent lubricity as claimed in claim 1, characterized in that: In step S3, the alcohol is at least one of ethylene glycol, ethanol, propanol, propylene glycol or butanediol; and / or The catalyst in step S2 and step S3 is one or a combination of two or more of sulfamic acid, p-toluenesulfonic acid and fluoroboric acid; and / or The reaction atmosphere of step S2 and step S3 is one of air, nitrogen and argon.
7. The method for preparing a palm polyol ester having good thermal stability and excellent lubricity as claimed in claim 1, characterized in that: In the step S3, the molar ratio of the palm polyol to the alcohol is 1:(2.0-3.5); and / or The amount of the catalyst is 1% to 5% of the mass of the palm polyol; and / or The temperature of the esterification reaction is 70° C. to 110° C., and the reaction time is 3 h to 5 h.
8. The method for preparing a palm polyol ester having good thermal stability and excellent lubricity as claimed in claim 1, characterized in that: After the esterification reaction in step S3 is completed, the reaction product is washed with a saturated inorganic salt solution, and then extracted with an organic solvent, and the aqueous phase and the organic phase are separated by standing and stratifying. The organic phase obtained after removing the organic solvent is the palm polyol ester; and / or The saturated inorganic salt solution is one or a combination of two or more of a sodium carbonate solution, a sodium bicarbonate solution and a sodium chloride solution; and / or The organic solvent is one or a combination of two or more of ethyl acetate, dichloromethane and n-hexane.
9. A palm polyol ester having good thermal stability and excellent lubricity, characterized in that: The invention is prepared by the preparation method of the palm polyol ester with good thermal stability and excellent lubricity as described in any one of claims 1 to 8.
10. A vegetable oil-based lubricant, characterized in that: Use of the palm polyol ester prepared by the method for preparing the palm polyol ester with good thermal stability and excellent lubricity according to any one of claims 1 to 8 in lubricants; The palm polyol ester is used alone as the vegetable oil-based lubricant; or, the palm polyol ester is added to a base oil as a lubricant additive to form the vegetable oil-based lubricant.