Ester type ionomer resin as well as preparation method and application thereof

Ester ionomer resin with ethylene, unsaturated carboxylic acid metal salt and unsaturated carboxylic acid ester structure was prepared by solvent method, which solved the complex and impurity metal salt problems of acid ionomer resin preparation, and achieved simplification of the process. Cost reduction and excellent performance.

CN118909166APending Publication Date: 2024-11-08JIANGSU SAILBOAT PETROCHEMICAL CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410971933.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing preparation methods of acid-type ionomer resins are complex and difficult to remove impurities and metal salts, which affect product performance, and lack simple and low-cost ester-type ionomer resin preparation technology.

Method used

Ester ionomer resins with ethylene, unsaturated carboxylic acid metal salts and unsaturated carboxylic acid ester structures are prepared by solvent method to reduce or contain carboxylic acid structures, avoid acid addition and demetalization and purification steps, optimize the process flow and Reduce costs.

Benefits of technology

The preparation process is simplified, the cost is reduced, and the three waste emissions are reduced. In addition, there is no white spots after the ester ionomer resin is tableted, and the performance is excellent.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004953490210000071
    Figure BDA0004953490210000071
  • Figure BDA0004953490210000081
    Figure BDA0004953490210000081
  • Figure BDA0004953490210000091
    Figure BDA0004953490210000091
Patent Text Reader

Abstract

The invention provides ester type ionomer resin as well as a preparation method and application thereof. The structure of the ester type ionomer resin contains an ethylene structural unit, an unsaturated carboxylic acid metal salt structural unit and an unsaturated carboxylic ester structural unit, the content of unsaturated carboxylate radicals in the ester type ionomer resin is low, acid addition for metal removal is not needed in the preparation process, no impurity metal salt is generated, purification is not needed, the technological process is greatly optimized, the production cost is reduced, and emission of three wastes is reduced; meanwhile, the molar content of acid radicals in the ester type ionomer resin is low, white spots cannot appear after tabletting, and the comprehensive performance is quite excellent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of ionomers, and in particular relates to an ester type ionomer resin and a preparation method and application thereof. Background Art

[0002] Ionomer resin refers to a class of polymers containing metal ions. The molecular structure is based on a copolymer of ethylene and unsaturated carboxylic acid as the main chain, on which metal ions are introduced, and ionic bonds are used as cross-links between molecules. It has excellent transparency, abrasion and scratch resistance, low-temperature impact toughness, chemical resistance and other advantages. It is widely used in sports equipment such as golf balls, bowling balls, sleds, surfboards, containers for cosmetics and perfumes, food packaging (especially vacuum skin packaging), glass multilayers (high-rise, architectural photovoltaic glass), automotive parts and polar exploration equipment.

[0003] Common ionomer resins are all acidic ionomer resins. From the perspective of polymer structure, acidic ionomer resins are composed of ethylene structural units, unsaturated carboxylic acid structural units and unsaturated carboxylic acid metal salt structural units. Generally, the molar fraction of ethylene structural units is greater than 90%, and the molar fraction of unsaturated carboxylic acid metal salt structural units accounts for 20-80% of the total of unsaturated carboxylic acid structural units and unsaturated carboxylic acid metal salt structural units. Since the structure contains a large amount of carboxylic acid structures, it has a certain acidity. The conventional preparation method is mainly a saponification method. When preparing acidic ionomer resins by a saponification method, it generally includes three steps of saponification, acid demetallization and purification.

[0004] For example, CN115768803A discloses an ionomer resin comprising: a carboxylate unit (A), a carboxylic acid unit (B), a carboxylic acid neutralization unit (C) and an ethylene unit (D). Based on all the monomer units constituting the ionomer resin, the content of the carboxylate unit (A) is 0.01 to 1.8 mol %, and the total content of the carboxylate unit (A), the carboxylic acid unit (B), and the carboxylic acid neutralization unit (C) is 6 to 10 mol %. The carboxylic acid unit (B) and the carboxylic acid neutralization unit (C) are converted into methyl carboxylate units. When the polyethylene-converted molecular weight is determined by GPC, the ratio of low molecular weight components with a molecular weight of less than 2500 g / mol obtained from the integrated molecular weight distribution curve is 2.6 to 4.0 mass %, and the number average molecular weight is 8000 to 14000 g / mol.

[0005] However, it can be seen that the preparation method of the acid-type ionomer resin has many steps, especially the purification step is very difficult, resulting in the presence of impurity metal salts in the obtained acid-type ionomer resin, which in turn affects the performance of the product; ester-type ionomer resin can effectively solve the above problems, but there are few reports on ester-type ionomers and their preparation and application in the prior art.

[0006] Therefore, it is of great significance to develop an ester-type ionomer resin with simple preparation process, low cost and excellent performance. Summary of the invention

[0007] In view of the deficiencies in the prior art, the object of the present invention is to provide an ester-type ionomer resin and a preparation method and application thereof. The structure of the alkaline ionomer resin contains ethylene structural units, unsaturated carboxylic acid metal salt structural units and unsaturated carboxylic acid ester structural units, and contains very small amounts (<1 mol%) or even no carboxylic acid structural units. Furthermore, the preparation process does not require purification, which greatly optimizes the process flow and reduces the preparation cost. No white spots will appear after tableting, and the performance is very excellent.

[0008] To achieve this object, the present invention adopts the following technical solutions:

[0009] In a first aspect, the present invention provides an ester type ionomer resin, wherein the structure of the ester type ionomer resin comprises ethylene structural units, unsaturated carboxylic acid metal salt structural units and unsaturated carboxylic acid ester structural units.

[0010] The structure of the ester type ionomer resin provided by the present invention contains ethylene structural units, unsaturated carboxylic acid metal salt structural units and unsaturated carboxylic acid ester structural units, and contains very little (<1 mol%) or even no unsaturated carboxylic acid structural units. Compared with conventional acid type ionomer resins, the ester type ionomer resin does not need to be demetallated by adding acid during the preparation process, and no impurity metal salt is generated, and no purification is required, which greatly optimizes the process flow, reduces costs, and reduces the discharge of three wastes. At the same time, the ester type ionomer resin will not have white spots after being pressed into tablets, and the comprehensive performance is very excellent.

[0011] Wherein, the structural formula of the ethylene structural unit is

[0012] Preferably, the molar ratio of the ethylene structural unit, the unsaturated carboxylic acid metal salt structural unit and the unsaturated carboxylic acid ester structural unit is 1:(0.05-0.95):(0.95-0.05), for example, 1:0.05:0.95, 1:0.1:0.9, 1:0.2:0.8, 1:0.3:0.7, 1:0.4:0.6, 1:0.5:0.5, 1:0.6:0.4, 1:0.7:0.3, 1:0.8:0.2, 1:0.9:0.1 or 1:0.95:0.05, etc., more preferably 1:(0.1-0.9):(0.9-0.1), and even more preferably 1:(0.2-0.8):(0.8-0.2).

[0013] Preferably, the unsaturated carboxylic acid metal salt structural unit includes a methacrylic acid metal salt structural unit and / or an acrylic acid metal salt structural unit, and more preferably an acrylic acid metal salt structural unit.

[0014] Wherein, the structural formula of the metal methacrylate structural unit is: The structural formula of the acrylic acid metal salt structural unit is: M represents an alkali metal element, such as Na, K, etc.

[0015] Preferably, the unsaturated carboxylic acid ester structural unit includes a butyl methacrylate structural unit and / or a butyl acrylate structural unit, and more preferably a butyl acrylate structural unit.

[0016] Wherein, the structural formula of the butyl methacrylate structural unit is: The chemical formula of the butyl acrylate structural unit is:

[0017] Preferably, the saponification degree of the unsaturated carboxylic acid ester in the ester type ionomer resin is 5-95%, for example, 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 50%, 60%, 70%, 80%, 90% or 95%, etc.

[0018] In the present invention, the saponification degree is obtained by FTIR-ATR characterization. The specific method is: the ester type ionomer resin and the ethylene-unsaturated carboxylic acid ester copolymer are tested by an infrared tester with a scanning range of 400 to 4000 cm -1 , resolution 4cm -1 , scanning times 32 times; the ester type ionomer resin was tested at 1735cm in the infrared spectrum. -1 The peak area at (corresponding to the stretching vibration peak of the C=O double bond in the ester group) is recorded as A1, and the ester type ionomer resin is obtained in the infrared spectrum at 3000-2800 m -1 The peak area at 1735 cm-1 in the infrared spectrum of the ethylene-unsaturated carboxylic acid ester copolymer was recorded as A2. -1 The peak area at 3000-2800 cm-1 in the infrared spectrum of the ethylene-unsaturated carboxylic acid ester copolymer was recorded as S1. -1 The peak area at (corresponding to the CH stretching vibration peak) is recorded as S2, and the saponification degree is finally calculated according to saponification degree = 1-A1 / A2 / (S1 / S2)×100%.

[0019] Preferably, the molar percentage of unsaturated carboxylate in the ester type ionomer resin is less than 1%, such as 0.9%, 0.8%, 0.7%, 0.6% or 0.5%.

[0020] In the present invention, the unsaturated carboxylate radical is obtained by ionization of unsaturated carboxylic acid metal salt units, and its molar percentage content is obtained by infrared spectroscopy.

[0021] In a second aspect, the present invention provides a method for preparing the ester type ionomer resin as described in the first aspect, the preparation method comprising: reacting an ethylene-unsaturated carboxylic acid ester copolymer, a base and a mixed solvent, and drying to obtain the ester type ionomer resin.

[0022] The preparation method of the ester type ionomer resin provided by the present invention is a solvent method, which uses an ethylene-unsaturated carboxylic acid ester copolymer as a base resin, saponifies the resin in the form of a solution by adding alkali, and obtains the resin by post-treatment and drying. Compared with the conventional solution method for preparing the acid type ionomer resin, it does not need to add acid for demetallization, does not generate impurity metal salts, and does not need purification, which greatly optimizes the process flow, reduces costs, and reduces the discharge of three wastes.

[0023] Preferably, based on the total mass of the ethylene-unsaturated carboxylate copolymer, the base and the mixed solvent as 100%, the mass of the ethylene-unsaturated carboxylate copolymer is 10-50%, for example 10%, 20%, 30%, 40% or 50%.

[0024] Preferably, the mass percentage of the unsaturated carboxylate structural unit in the ethylene-unsaturated carboxylate copolymer is 7-35%, for example, 7%, 10%, 15%, 20%, 25%, 30% or 35%.

[0025] Preferably, the melt index of the ethylene-unsaturated carboxylate copolymer is 5 to 300 g / 100 min, for example, 5 g / 100 min, 10 g / 100 min, 50 g / 100 min, 100 g / 100 min, 150 g / 100 min, 200 g / 100 min, 250 g / 100 min or 300 g / 100 min, and more preferably 20 to 150 g / 10 min; the test temperature of the above melt index is 190° C. and the load is 2.16 kg.

[0026] Preferably, the ethylene-unsaturated carboxylic acid ester copolymer includes ethylene-butyl acrylate copolymer and / or ethylene-methyl methacrylate copolymer, and more preferably ethylene-butyl acrylate copolymer.

[0027] Preferably, the molar ratio of the ethylene-unsaturated carboxylic acid ester copolymer to the base is 1:(0.05-0.95), for example, 1:0.05, 1:0.1, 1:0.2, 1:0.3, 1:0.4, 1:0.5, 1:0.6, 1:0.7, 1:0.8, 1:0.9 or 1:0.95, etc., more preferably 1:(0.1-0.9), and even more preferably 1:(0.2-0.8).

[0028] Preferably, the alkali comprises sodium hydroxide and / or potassium hydroxide, more preferably sodium hydroxide.

[0029] Preferably, the mixed solvent is a mixture of an alcohol solvent and an aromatic solvent.

[0030] Preferably, the mass ratio of the alcohol solvent to the aromatic solvent is (1-3):(9-7), such as 1:9, 2:8 or 3:7.

[0031] Preferably, the alcohol solvent includes any one of methanol, ethanol, tert-butanol, n-butanol or isopropanol, or a combination of at least two thereof, and methanol is more preferably used.

[0032] Preferably, the aromatic solvent includes any one of p-xylene, o-xylene, m-xylene, xylene, and toluene, or a combination of at least two of them, and more preferably xylene and / or p-xylene.

[0033] Preferably, the reaction temperature is ≥150°C, for example 150°C, 155°C, 160°C, 165°C, 170°C, 175°C, 180°C, 185°C, 190°C, 195°C or 200°C, etc., more preferably ≥160°C, and even more preferably ≥180°C.

[0034] Preferably, the reaction time is 0.5 to 6 h, for example 0.5 h, 1 h, 2 h, 3 h, 4 h, 5 h or 6 h.

[0035] Preferably, the reaction pressure is 0-10 MPa, such as 0 MPa, 2 MPa, 4 MPa, 6 MPa, 8 MPa or 10 MPa.

[0036] In a third aspect, the present invention provides a use of the ester ionomer resin as described in the first aspect in the preparation of sports equipment, cosmetic containers, perfume containers, food packaging materials, glass laminates, automotive parts or polar exploration equipment.

[0037] Compared with the prior art, the present invention has the following beneficial effects:

[0038] (1) The structure of the ester type ionomer resin provided by the present invention contains ethylene structural units, unsaturated carboxylic acid metal salt structural units and unsaturated carboxylic acid ester structural units; the structure of the ester type ionomer resin contains very little (<1 mol%) or even no unsaturated carboxylic acid structural units, and thus, compared with the acid type ionomer resin, the ester type ionomer resin does not need to be demetallated by adding acid during the preparation process, no impurity metal salt is generated, and no purification is required, which greatly optimizes the process flow, reduces costs, and reduces the discharge of three wastes.

[0039] (2) The ester-type ionomer resin provided by the present invention also has high transparency, no white spots will appear after tableting, and the overall performance is very excellent. DETAILED DESCRIPTION

[0040] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0041] The detailed information of some raw materials involved in the following examples and comparative examples are as follows:

[0042] (1) Ethylene-butyl acrylate copolymer (EnBA):

[0043] EnBA20020: melt index is 20 g / 10 min, 190°C, the mass percentage of butyl acrylate structural unit is 20%, purchased from Repsol, brand name E20020;

[0044] EnBA27150: melt index is 150 g / 10 min, 190°C, the mass percentage of butyl acrylate structural unit is 27%, purchased from Repsol, brand E27150;

[0045] EnBA33150: melt index is 150 g / 10 min, 190° C., the mass percentage of butyl acrylate structural unit is 33%, purchased from Repsol, brand number E33150.

[0046] (2) Anhydrous methanol: AR grade, Sinopharm Reagent.

[0047] (3) p-Xylene: AR grade, Sinopharm Reagent.

[0048] (3) Sodium hydroxide: NaOH, AR grade, Sinopharm Reagent.

[0049] Example 1

[0050] An ester type ionomer resin comprises an ethylene structural unit as shown in formula I, an acrylic acid sodium salt structural unit as shown in formula II, and a butyl acrylate structural unit as shown in formula III:

[0051]

[0052] Wherein, the molar ratio of the ethylene structural unit represented by formula I, the sodium acrylate structural unit represented by formula II and the butyl acrylate structural unit represented by formula III is 1:0.6:0.4;

[0053] The preparation method of the ester ionomer resin provided in this embodiment includes: placing 25.8g of ethylene-butyl acrylate copolymer EnBA20020, 48g of p-xylene, 12g of methanol and 1.0g of sodium hydroxide in a reactor, stirring and heating to 180°C, reacting at 2MPa for 1h and then terminating the reaction, and drying to obtain the ester ionomer resin.

[0054] Example 2

[0055] An ester type ionomer resin, which differs from Example 1 in that the reaction temperature is 160° C. and the reaction time is 2 hours, and other structures, materials and parameters are the same as those of Example 1.

[0056] Example 3

[0057] An ester type ionomer resin is different from Example 1 in that the reaction temperature is 150° C. and the reaction time is 4 hours. Other structures, materials and parameters are the same as those in Example 1.

[0058] Example 4

[0059] An ionomer resin comprises an ethylene structural unit as shown in formula I, an acrylic acid sodium salt structural unit as shown in formula II, and a butyl acrylate structural unit as shown in formula III:

[0060]

[0061] Wherein, the molar ratio of the structural unit represented by formula I, the sodium acrylate structural unit represented by formula II and the butyl acrylate structural unit represented by formula III is 1:0.8:0.2;

[0062] The preparation method of the ester ionomer resin provided in this embodiment includes: placing 25.8g of ethylene-butyl acrylate copolymer EnBA27150, 48g of p-xylene, 12g of methanol and 1.7g of sodium hydroxide in a reactor, stirring and heating to 180°C, reacting at 2MPa for 4h and then terminating the reaction, and drying to obtain the ester ionomer resin.

[0063] Example 5

[0064] An ionomer resin comprises an ethylene structural unit represented by formula I, an acrylic acid sodium salt structural unit represented by formula II, and a butyl acrylate structural unit represented by formula III:

[0065]

[0066] Wherein, the molar ratio of the structural unit represented by formula I, the sodium acrylate structural unit represented by formula II and the butyl acrylate structural unit represented by formula III is 1:0.5:0.5;

[0067] The preparation method of the ester ionomer resin provided in this embodiment includes: placing 30g of ethylene-butyl acrylate copolymer EnBA27150, 24g of p-xylene, 6g of methanol and 1.3g of sodium hydroxide in a reactor, stirring and heating to 180°C, reacting at 3MPa for 2h and then terminating the reaction, and drying to obtain the ester ionomer resin.

[0068] Example 6

[0069] An ionomer resin comprises an ethylene structural unit as shown in formula I, an acrylic acid sodium salt structural unit as shown in formula II, and a butyl acrylate structural unit as shown in formula III:

[0070]

[0071] Wherein, the molar ratio of the structural unit represented by formula I, the sodium acrylate structural unit represented by formula II and the butyl acrylate structural unit represented by formula III is 1:0.5:0.5;

[0072] The preparation method of the ester ionomer resin provided in this embodiment includes: placing 7g of ethylene-butyl acrylate copolymer EnBA27150, 50.4g of p-xylene, 12.6g of methanol and 0.3g of sodium hydroxide in a reactor, stirring and heating to 150°C, reacting at 2MPa for 2h and then terminating the reaction, and drying to obtain the ester ionomer resin.

[0073] Example 7

[0074] An ionomer resin comprises an ethylene structural unit shown in formula I, an acrylic acid sodium salt structural unit shown in formula II, and a butyl acrylate structural unit shown in formula III:

[0075]

[0076] Wherein, the molar ratio of the structural unit represented by formula I, the sodium acrylate structural unit represented by formula II and the butyl acrylate structural unit represented by formula III is 1:0.1:0.9;

[0077] The preparation method of the ester ionomer resin provided in this embodiment includes: placing 25.8g of ethylene-butyl acrylate copolymer EnBA33150, 24g of p-xylene, 36g of methanol and 0.3g of sodium hydroxide in a reactor, stirring and heating to 180°C, reacting at 1MPa for 4h and then terminating the reaction, and drying to obtain the ester ionomer resin.

[0078] Example 8

[0079] An ionomer resin, which differs from Example 1 in that the molar ratio of the structural unit represented by formula I, the sodium acrylate structural unit represented by formula II and the butyl acrylate structural unit represented by formula III is 1:0.3:0.7, the amount of sodium hydroxide used in the preparation method is 0.5 g, and other substances, amounts and parameters are the same as those in Example 1.

[0080] Example 9

[0081] An ester type ionomer resin comprises an ethylene structural unit as shown in formula I, an acrylic acid sodium salt structural unit as shown in formula II, and a butyl acrylate structural unit as shown in formula III:

[0082]

[0083] Wherein, the molar ratio of the ethylene structural unit represented by formula I, the sodium acrylate structural unit represented by formula II and the butyl acrylate structural unit represented by formula III is 1:0.4:0.6;

[0084] The preparation method of the ester ionomer resin provided in this embodiment includes: placing 25.8g of ethylene-butyl acrylate copolymer EnBA20020, 48g of xylene, 12g of methanol and 0.6g of sodium hydroxide in a reactor, stirring and heating to 180°C, reacting at 1MPa for 2h and then terminating the reaction, and drying to obtain the ester ionomer resin.

[0085] Example 10

[0086] An ester type ionomer resin is different from Example 1 in that the molar ratio of the structural unit represented by Formula I, the sodium acrylate structural unit represented by Formula II and the butyl acrylate structural unit represented by Formula III is 1:0.5:0.5, the amount of sodium hydroxide used in the preparation method is 0.8 g, and other substances, amounts and parameters are the same as those in Example 1.

[0087] Embodiment 11

[0088] An ester type ionomer resin is different from Example 1 in that the reaction temperature is 140° C. and the reaction time is 2 hours. Other substances, amounts and parameters are the same as those in Example 1.

[0089] Example 12

[0090] An ester type ionomer resin is different from Example 1 in that the reaction temperature is 120° C. and the reaction time is 4 hours. Other substances, amounts and parameters are the same as those in Example 1.

[0091] Comparative Example 1

[0092] An ionomer resin, the preparation method of which comprises: placing 25.8g of ethylene-butyl acrylate copolymer EnBA20020, 48g of p-xylene, 12g of methanol and 1.7g of sodium hydroxide in a reactor, stirring and heating to 180°C, reacting at 2MPa for 1h and then terminating the reaction, and drying to obtain the ionomer resin.

[0093] Performance Testing:

[0094] (1) Saponification degree: obtained by FTIR-ATR characterization. The specific method is as follows: the ionomer resin and ethylene-butyl acrylate copolymer were tested using an infrared tester with a scanning range of 400 to 4000 cm -1 , resolution 4cm -1 , scanning times 32 times; the test shows that the ionomer resin has a peak at 1735cm in the infrared spectrum. -1 The peak area at (corresponding to the stretching vibration peak of the C=O double bond in the ester group) is recorded as A1, and the ester type ionomer resin is obtained in the infrared spectrum at 3000-2800 m -1 The peak area at 1735 cm-1 in the infrared spectrum of the ethylene-unsaturated carboxylic acid ester copolymer was recorded as A2. -1 The peak area at 3000-2800 cm-1 in the infrared spectrum of the ethylene-unsaturated carboxylic acid ester copolymer was recorded as S1. -1 The peak area at (corresponding to the CH stretching vibration peak) is recorded as S; finally, the saponification degree is calculated according to saponification degree = 1-A1 / A2 / (S1 / S2)×100%.

[0095] (2) Acid radical molar content: The ionomer resin is tested using an infrared spectrometer. If the ionomer resin has a molar content of 1700 cm-1 in the infrared spectrum, -1 There is no peak at , which means the molar content of acid radical is less than 1%.

[0096] (3) White spots on tablets: The ionomer resin was tableted at 180° C. and 30 MPa for 5 min to obtain an ionomer resin sheet with a thickness of 0.5 mm. The sheet was visually observed for white spots.

[0097] The ionomer resins provided in Examples 1 to 12 and Comparative Example 1 were tested according to the above test method. The test results are shown in Table 1:

[0098] Table 1

[0099] Serial number NaOH equivalent Saponification degree / % Acid radical molar content / % White spots on tablets Example 1 0.6 60 <1 No white spots Example 2 0.6 60 <1 No white spots Example 3 0.6 60 <1 No white spots Example 4 0.8 80 <1 No white spots Example 5 0.5 50 <1 No white spots Example 6 0.5 50 <1 No white spots Example 7 0.1 10 <1 No white spots Example 8 0.3 30 <1 No white spots Example 9 0.4 40 <1 No white spots Example 10 0.5 50 <1 No white spots Embodiment 11 0.6 50 <1 A small amount of white spots Example 12 0.6 25 <1 Lots of white spots Comparative Example 1 1.05 >99.5 <1 Lots of white spots

[0100] From the data in Table 1, we can see that:

[0101] The saponification degree of the ester type ionomer resin provided in Examples 1 to 10 is 10 to 80%, the acid group molar content is less than 1%, and no white spots appear after tableting, while the saponification degree of the ionomer resin provided in Comparative Example 1 is as high as 99.5%, and a large number of white spots appear after tableting;

[0102] By comparing the data of Example 1 with those of Examples 11 to 12, it can be found that the reaction temperature also affects the performance of the final ester-type ionomer resin. Too low a reaction temperature will also lead to white spots on the ionomer resin after tableting.

[0103] The applicant declares that the present invention illustrates an ester type ionomer resin and its preparation method and application through the above embodiments, but the present invention is not limited to the above embodiments, that is, it does not mean that the present invention must rely on the above embodiments to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. An ester type ionomer resin, characterized in that The structure of the ester type ionomer resin contains ethylene structural units, unsaturated carboxylic acid metal salt structural units and unsaturated carboxylic acid ester structural units.

2. The ester type ionomer resin according to claim 1, characterized in that The molar ratio of the ethylene structural unit, the unsaturated carboxylic acid metal salt structural unit and the unsaturated carboxylic acid ester structural unit is 1:(0.05-0.95):(0.95-0.05), preferably 1:(0.1-0.9):(0.9-0.1), and more preferably 1:(0.2-0.8):(0.8-0.2).

3. The ester type ionomer resin according to claim 1 or 2, characterized in that: The unsaturated carboxylic acid metal salt structural unit comprises a methacrylic acid metal salt structural unit and / or an acrylic acid metal salt structural unit, preferably an acrylic acid metal salt structural unit; Preferably, the unsaturated carboxylic acid ester structural unit includes a butyl methacrylate structural unit and / or a butyl acrylate structural unit, and more preferably a butyl acrylate structural unit.

4. The ester type ionomer resin according to any one of claims 1 to 3, characterized in that: The saponification degree of the unsaturated carboxylic acid ester in the ester type ionomer resin is 5 to 95%; Preferably, the molar percentage of unsaturated carboxylate in the ester type ionomer resin is less than 1%.

5. A method for preparing the ester type ionomer resin according to any one of claims 1 to 4, characterized in that: The preparation method comprises: reacting ethylene-unsaturated carboxylic acid ester copolymer, alkali and mixed solvent, and drying to obtain the ester type ionomer resin.

6. The preparation method according to claim 5, characterized in that: Based on the total mass of the ethylene-unsaturated carboxylate copolymer, the base and the mixed solvent as 100%, the mass of the ethylene-unsaturated carboxylate copolymer is 10 to 50%; Preferably, the mass percentage of the unsaturated carboxylate structural unit in the ethylene-unsaturated carboxylate copolymer is 7 to 35%; Preferably, the melt index of the ethylene-unsaturated carboxylic acid ester copolymer is 5 to 300 g / 100 min, more preferably 20 to 150 g / 10 min; Preferably, the ethylene-unsaturated carboxylic acid ester copolymer includes ethylene-butyl acrylate copolymer and / or ethylene-methyl methacrylate copolymer, and more preferably ethylene-butyl acrylate copolymer.

7. The preparation method according to claim 5 or 6, characterized in that: The molar ratio of the ethylene-unsaturated carboxylic acid ester copolymer to the base is 1:(0.05-0.95), preferably 1:(0.1-0.9), and more preferably 1:(0.2-0.8); Preferably, the base comprises sodium hydroxide and / or potassium hydroxide, preferably sodium hydroxide.

8. The preparation method according to claims 5 to 7, characterized in that: The mixed solvent is a mixture of an alcohol solvent and an aromatic solvent; Preferably, the mass ratio of the alcohol solvent to the aromatic solvent is (1-3):(9-7); Preferably, the alcohol solvent includes any one of methanol, ethanol, tert-butanol, n-butanol or isopropanol, or a combination of at least two thereof, and methanol is more preferably used; Preferably, the aromatic solvent includes any one of p-xylene, o-xylene, m-xylene, xylene, and toluene, or a combination of at least two of them, and more preferably xylene and / or p-xylene.

9. The preparation method according to any one of claims 5 to 8, characterized in that: The reaction temperature is ≥150°C, preferably ≥160°C, and more preferably ≥180°C; Preferably, the reaction time is 0.5 to 6 hours; Preferably, the reaction pressure is 0-10 MPa.

10. Use of the ester ionomer resin according to any one of claims 1 to 4 in the preparation of sports equipment, cosmetic containers, perfume containers, food packaging materials, glass laminates, automobile parts or polar exploration equipment.