Method for rapidly preparing nanoscale short dendrite SiC
Through the method of rapid heating and cooling of Joule heat, combined with multiple thermal cycles, the preparation process of nano-scale short-branched crystal SiC is simplified, and the problems of long preparation cycles and complex equipment in the existing technology are solved, achieving high efficiency and low cost Nanoscale short-branched crystal SiC preparation, suitable for large-scale production.
Patent Information
- Application Number
- CN202411442479.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-16
- Publication Date
- 2024-12-06
AI Technical Summary
The existing nano-scale short-branched crystal SiC synthesis methods have problems such as long preparation cycle, complex equipment and high cost, and it is difficult to meet the high-efficiency and low-cost preparation needs.
By using Joule heat for rapid heating and cooling, combined with multiple thermal cycles, the process flow is simplified to prepare nano-scale short-branched crystal SiC that meets the needs. Specific steps include mixing the powder, vacuum treatment, heating and insulation, rapid cooling and repeated thermal cycles, and finally cooling to room temperature.
It significantly shortens the SiC nucleation and growth time, is simple in process and low in cost, is suitable for large-scale production, and prepares uniform nano-scale short-branched SiC, which improves material performance and application prospects.
Smart Images

Figure CN119079999A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of nanotechnology, in particular to a method for rapidly preparing nanoscale short-branched SiC. Background Art
[0002] Silicon carbide (SiC) is a wide bandgap semiconductor material with excellent performance. It has high hardness close to diamond, a melting point of about 2700℃, high corrosion resistance, high thermal conductivity of 120-270W / m·K and good mechanical strength. These characteristics make it widely used in aerospace, electronic devices, mechanical seals and coatings. On this basis, nano-scale short-branched SiC, as an emerging material, shows more superior comprehensive performance, especially in the enhancement and functionalization of composite materials. It has great application potential. Compared with traditional micron-sized SiC particles, nano-scale short-branched SiC has a larger specific surface area and higher surface activity, giving it stronger interfacial bonding in composite materials. Its short-branched structure can play a bridge role in stress transfer in composite materials, significantly improving the mechanical strength and toughness of the material. In addition, the size effect of nano-SiC significantly improves the thermal conductivity and electrical properties of the material. In high-performance ceramic-based composites, metal-based composites and high-temperature anti-oxidation coatings, nano-scale short-branched SiC shows great application prospects. For example, adding nano-scale short-branched SiC to carbon-based composites can improve the thermal shock resistance, mechanical properties and oxidation resistance of the material, significantly extending its service life in high temperature and extreme environments. Such composite materials have broad application potential in the manufacture of high-temperature structural parts such as aerospace thermal protection systems, engine components, and turbine blades.
[0003] At present, the methods for synthesizing nanoscale short-branched SiC include sol-gel method, chemical vapor deposition (CVD) method and carbon thermal reduction method. Among them, the sol-gel method includes multiple steps, such as hydrolysis, polycondensation, gelation and heat treatment. The whole process cycle is long (about 3-5 days), the process is complex, and the temperature, humidity, reaction time and chemical reagent dosage need to be strictly controlled, and the operation requirements are high. When preparing short-branched SiC by CVD method, the cycle is relatively long. The typical process includes preheating of the reaction chamber (1-2 hours), reaction deposition (several hours to tens of hours), and cooling after the reaction (several hours). The whole process usually takes 8-24 hours from preparation to completion. The CVD method has complex equipment and high cost. It requires high-precision control of gas flow, temperature and pressure. The commonly used precursor gases in the process, such as methyltrichlorosilane, dichlorodimethylsilane and silane, are toxic or corrosive. If the operation is improper, it may pose a threat to the health of the experimenters. At the same time, a strict gas treatment system is required. In addition, it is not easy to prepare uniform short-branched SiC by CVD method. The carbon thermal reduction method has a long cycle for preparing nano-scale short-branched SiC, which usually requires multiple steps such as precursor preparation, carbon thermal reduction reaction and furnace cooling. The whole process takes about 18-40 hours, and the size distribution of the obtained SiC particles is large, which is difficult to meet the requirements of nano-scale short-branched SiC.
[0004] Therefore, developing an efficient and low-cost method for preparing nanoscale short-branched SiC has become the key to improving material properties and promoting the development of related application fields. Summary of the invention
[0005] The present invention provides a method for rapidly preparing nanoscale short-branched SiC to solve the problems of long preparation cycle, complex equipment and high cost in the current synthesis method of nanoscale short-branched SiC. The present invention realizes efficient preparation of nanoscale short-branched SiC in a very short time by utilizing the Joule heat generated when the material is energized. The method has the advantage of low energy consumption, and effectively suppresses the lateral growth of SiC grains through the rapid heating and cooling process, thereby preparing nanoscale short-branched SiC that meets the requirements.
[0006] A method for rapidly preparing nanoscale short-branched SiC comprises the following steps:
[0007] 1) Mixing powder: mixing the silicon source and the carbon source to obtain a uniform mixed powder;
[0008] 2) Loading the electrode container and evacuating: Loading the mixed powder into a container with an electrode, and then placing the electrode on a sample holder in a Joule heating furnace, and then turning on a vacuum pump to evacuate the cavity;
[0009] 3) Heating and keeping warm: using Joule heat to heat the blank to the target temperature and keep it warm for a period of time;
[0010] 4) Rapid cooling and heat preservation: Rapidly reduce the temperature to 1000-1500℃, keep it warm for 5-20s, and complete a thermal cycle;
[0011] 5) Repeating the thermal cycle: Repeat the thermal cycle of the above steps 3) and 4) for several times, and finally cool to room temperature to obtain nano-scale short-branched SiC.
[0012] As a preferred solution, in step 1), the silicon source is at least one of nano-silicon powder and silicon monoxide, and the carbon source is at least one of graphene and carbon nanotubes.
[0013] As a preferred embodiment, in step 1), the molar ratio of the silicon source to the carbon source is 1:1-2.
[0014] As a preferred solution, the vacuum degree of the vacuum in step 2) is 0.05-0.2 Pa.
[0015] As a preferred solution, in step 3), the blank is heated to 1300-1700°C.
[0016] As a preferred solution, in step 3), the blank is heated to the target temperature and then kept warm for 5 to 20 seconds.
[0017] As a preferred solution, the temperature difference in each thermal cycle in step 5) is 200-300°C.
[0018] As a preferred embodiment, the thermal cycle in step 5) is repeated 1 to 5 times.
[0019] The advantages of the present invention compared with the prior art are: by utilizing the rapid heating and cooling characteristics of Joule heat, the time required for SiC nucleation and growth is significantly shortened. Compared with the long heating process of the traditional electric furnace, the present invention can complete the nucleation and growth of SiC within a few seconds to tens of seconds. The initial high temperature in the step-by-step heating process is conducive to the rapid nucleation of SiC, and the large temperature difference causes atmosphere fluctuations, providing ideal conditions for the growth of branched structure. In addition, by adjusting the number of thermal cycles, the aspect ratio of short branched SiC can be controlled. The process is simple, low-cost, and suitable for large-scale production, and has significant application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is a high-magnification scanning image of the short-branched SiC obtained in Example 1;
[0021] Figure 2 This is a low-magnification scanning image of the short-branched SiC obtained in Example 1;
[0022] Figure 3 This is a statistical diagram of the diameter of short branched SiC obtained in Example 1;
[0023] Figure 4 This is a length statistical diagram of short branched SiC obtained in Example 1;
[0024] Figure 5 This is a high-magnification scanning image of the short-branched SiC obtained in Example 2;
[0025] Figure 6 This is a low-magnification scanning image of the short-branched SiC obtained in Example 2;
[0026] Figure 7 This is a statistical diagram of the diameter of short branched SiC obtained in Example 2;
[0027] Figure 8 This is a length statistical diagram of short branched SiC obtained in Example 2. DETAILED DESCRIPTION
[0028] The technical solution of the present invention is not limited to the specific implementation modes listed below, but also includes any reasonable combination of the specific implementation modes.
[0029] A method for rapidly preparing nanoscale short-branched SiC comprises the following steps:
[0030] 1) Mixed powder: a silicon source and a carbon source are mixed to obtain a uniform mixed powder, wherein the silicon source is at least one of nano silicon powder and silicon monoxide, the carbon source is at least one of graphene and carbon nanotubes, and the molar ratio of the silicon source to the carbon source is 1:1 to 2;
[0031] 2) Loading the electrode container and evacuating: Load the mixed powder into a container with an electrode, then place the electrode on a sample holder in a Joule heating furnace, and then start the vacuum pump to evacuate the cavity to a vacuum degree of 0.05-0.2 Pa;
[0032] 3) Heating and keeping warm: using Joule heat to heat the blank to 1300-1700°C and keep warm for 5-20s;
[0033] 4) Rapid cooling and heat preservation: Rapidly reduce the temperature to 1000-1500℃, keep it warm for 5-20s, and complete a thermal cycle;
[0034] 5) Repeating the thermal cycle: Repeat the thermal cycle of the above steps 3) and 4 for 1 to 5 times, with a temperature difference of 200 to 300° C. for each thermal cycle, and finally cool to room temperature to obtain nanoscale short-branched SiC.
[0035] Embodiment 1
[0036] A method for rapidly preparing nanoscale short-branched SiC is to follow the following steps:
[0037] Nano-silicon powder and graphene are mixed in a molar ratio of 1:1 to obtain a uniform mixed powder; the mixed powder is loaded into a container with an electrode, and then the electrode is placed on a sample holder in a Joule heating furnace, and then the vacuum pump is turned on to evacuate the cavity to 0.1 Pa; the blank is heated to 1600°C using Joule heat and kept warm for 5 seconds; then, the temperature is quickly reduced to 1400°C and kept warm for 10 seconds to complete a thermal cycle; after completing one cycle, the thermal cycle is repeated 3 times, and finally cooled to room temperature to obtain nano-scale short-branched SiC.
[0038] This embodiment has the following beneficial effects:
[0039] The nanoscale short-branched SiC obtained in Example 1 is as follows Figure 1 and Figure 2 As shown, the diameter statistics and length statistics are as follows Figure 3 and Figure 4 As shown, the product presents an obvious branched crystal structure and is relatively uniform in morphology, with an average diameter of 150nm, an average length of 434nm, an aspect ratio of about 3:1, a diameter distribution of 50 to 350nm, and a small size distribution. The process is simple and low in cost, and nanoscale short branched SiC can be efficiently prepared in a very short time (<60s).
[0040] Embodiment 2
[0041] A method for rapidly preparing nanoscale short-branched SiC is to follow the following steps:
[0042] Nano-silicon powder and carbon nanotubes are mixed in a molar ratio of 1:1.5 to obtain a uniform mixed powder; the mixed powder is loaded into a container with an electrode, and then the electrode is placed on a sample holder in a Joule heating furnace, and then a vacuum pump is turned on to evacuate the cavity to 0.2 Pa; the blank is heated to 1500°C using Joule heat and kept warm for 30 seconds; then, the temperature is quickly reduced to 1100°C and kept warm for 15 seconds to complete a thermal cycle; after completing one cycle, the thermal cycle is repeated 5 times, and finally cooled to room temperature to obtain nano-scale short-branched SiC.
[0043] This embodiment has the following beneficial effects:
[0044] The nanoscale short-branched SiC obtained in Example 2 is as follows Figure 5 and Figure 6 As shown, the diameter statistics and length statistics are as follows Figure 7 and Figure 8 As shown, the product presents an obvious branched crystal structure, with an average diameter of 64nm, an average length of 652nm, an aspect ratio of about 10:1, a diameter distribution of 20 to 160nm, and a small size distribution. The process is simple and low-cost, and nano-scale short-branched SiC can be efficiently prepared in a very short time.
[0045] The present invention and its embodiments are described above, which is not restrictive. The drawings show only one embodiment of the present invention, and the actual structure is not limited thereto. In short, if ordinary technicians in the field are inspired by it and do not deviate from the purpose of the invention, they can creatively design a structure and embodiment similar to the technical solution, which should fall within the protection scope of the present invention.
Claims
1. A method for rapidly preparing nanoscale short-branched SiC, characterized in that: The specific steps include: 1) Mixing powder: mixing the silicon source and the carbon source to obtain a uniform mixed powder; 2) Loading the electrode container and evacuating: Load the mixed powder into a container with an electrode, then place the electrode on a sample holder in a Joule heating furnace, and then turn on the vacuum pump to evacuate the cavity; 3) Heating and keeping warm: using Joule heat to heat the blank to the target temperature and keep it warm for a period of time; 4) Rapid cooling and heat preservation: Rapidly reduce the temperature to 1000-1500℃, keep it warm for 5-20s, and complete a thermal cycle; 5) Repeating the thermal cycle: Repeat the thermal cycle of the above steps 3) and 4) for several times, and finally cool to room temperature to obtain nano-scale short-branched SiC.
2. A method for rapidly preparing nanoscale short-branched SiC according to claim 1, characterized in that: In the step 1), the silicon source is at least one of nano silicon powder and silicon monoxide, and the carbon source is at least one of graphene and carbon nanotubes.
3. The method for rapidly preparing nanoscale short-branched SiC according to claim 1, characterized in that: In the step 1), the molar ratio of the silicon source to the carbon source is 1:1-2.
4. The method for rapidly preparing nanoscale short-branched SiC according to claim 1, characterized in that: The vacuum degree of the vacuum pumping in the step 2) is 0.05-0.2 Pa.
5. The method for rapidly preparing nanoscale short-branched SiC according to claim 1, characterized in that: In the step 3), the blank is heated to 1300-1700°C.
6. The method for rapidly preparing nanoscale short-branched SiC according to claim 1, characterized in that: In the step 3), the blank is heated to the target temperature and then kept at the temperature for 5 to 20 seconds.
7. The method for rapidly preparing nanoscale short-branched SiC according to claim 1, characterized in that: The temperature difference in each thermal cycle in step 5) is 200-300°C.
8. The method for rapidly preparing nanoscale short-branched SiC according to claim 1, characterized in that: In step 5), the thermal cycle is repeated 1 to 5 times.
Citation Information
Patent Citations
Novel resistance-type ultrafast variable-temperature heating furnace and using method thereof
CN113340110A
Carbide and preparation method thereof
CN115403045A
Preparation method, application and preparation device of low-voltage and high-specific-capacity hard carbon
CN116443868A
Method for preparing silicon carbide material by taking silicon slag as raw material and application
CN118771383A
Method of coating carbon filaments with silicon carbide
US4131697A
Cited By