Polycarboxylic acid high-performance water reducing agent and synthesis method thereof
Through the polycarboxylic acid high-performance water reducing agent with block polymer structure, combined with water retention and water reduction blocks, the problem of insufficient adaptability of polycarboxylic acid water reducing agent to concrete materials is solved, and the concrete and ease is improved It can be used to avoid water leakage and ensure the quality of construction.
Patent Information
- Application Number
- CN202410953065.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-08
AI Technical Summary
Polycarboxylic acid high-performance water reducing agent can easily lead to separation, separation, and water leakage of concrete mixture when the amount is not added at the time, and it is sensitive to the aggregate sludge content, making it difficult to ensure the quality of concrete and the workingability during the construction process.
Polycarboxylic acid high-performance water reducing agent with block polymer structure is used, and unsaturated organic acid ester monomer, unsaturated acid monomer and unsaturated amide monomer respectively through the combination of water-retaining blocks and water-reducing blocks. The water reducing agent with excellent properties is prepared by a specific polymerization step.
Improve the ease and cohesion of concrete mixture, avoid water leakage and segregation, and ensure the working state and quality of concrete, especially when the grading of sand and gravel materials is unreasonable or the C3A content in cement is low. , reducing slump loss and hysteresis water discharge phenomenon.
Smart Images

Figure CN118909211A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of water reducing agents, and particularly relates to a polycarboxylic acid high-performance water reducing agent and a synthesis method thereof. Background Art
[0002] Polycarboxylic acid high-performance water-reducing agent is a new, green, environmentally friendly and efficient water-reducing agent with low dosage, high water-reducing rate, good cement adaptability, low slump loss, high early strength, high dispersibility and short retarding time. It is widely used in high-speed railway construction and various major projects. With the development of raw material synthesis technology, polycarboxylic acid high-performance water-reducing agent has been rapidly promoted to municipal engineering, civil construction and other markets with its improved performance, reduced cost and good application effect, and has been widely used.
[0003] However, in practical applications, polycarboxylate water reducer has the following technical difficulties:
[0004] (1) Due to the high water reducing property and material sensitivity of polycarboxylic acid high-performance water reducer, when the dosage is slightly high, it is easy to cause the concrete mixture to separate, segregate, bleed, and bleed, making the concrete mixture lose its workability; when the dosage is slightly low, the initial slump of the concrete mixture is small and the slump loss is serious, which makes it impossible to ensure the long-distance and pipeline transportation of concrete;
[0005] (2) Compared with naphthalene and aliphatic high-efficiency water reducers, polycarboxylic acid high-performance water reducers are more sensitive to the mud content of aggregates and are more easily adsorbed by mud in aggregates;
[0006] (3) Due to the widespread use of machine-made sand, the quality and gradation of machine-made sand are much different from those of river sand, and the gradation is unreasonable. For example, the amount of sand below 0.315 mm is too small, and the amount above 2.5 mm is too large. The cohesiveness of concrete is greatly affected, resulting in serious segregation and bleeding;
[0007] (4) Due to the control of cement production costs, when the C3A content in cement is low, the alkali content is low, the amount of admixture is large (especially mineral powder), the cement setting time is long, and delayed bleeding is prone to occur. When the inert material in cement is large, delayed bleeding is prone to occur.
[0008] The above problems eventually lead to many quality problems in the concrete construction process. Therefore, it is necessary to synthesize an environmentally friendly and high-performance polycarboxylic acid high-performance water reducer to solve the above problems. Summary of the invention
[0009] In view of the problems existing in the prior art, the purpose of the present invention is to provide a polycarboxylic acid high-performance water-reducing agent and a synthesis method thereof, which solves the adaptability of the existing polycarboxylic acid water-reducing agent to concrete materials such as cement and sand and gravel materials, and avoids the problems of poor concrete state and water seepage caused by poor quality of cement, sand and gravel.
[0010] The first aspect of the present invention provides a polycarboxylic acid high-performance water-reducing agent, which is a block polymer, consisting of a water-retaining block and a water-reducing block, and the mass ratio of the two is 1-2:2-1;
[0011] The raw material composition of the water-retaining block includes: unsaturated organic acid ester monomer, unsaturated acid monomer, unsaturated amide monomer, unsaturated sulfonate, and the mass ratio is (10-40): (10-30): (10-40): (5-10);
[0012] The raw material composition of the water-reducing block includes: unsaturated terminal polyoxyethylene ether monomer, unsaturated acid monomer, unsaturated organic acid hydroxy ester monomer, and the mass ratio is 100: (10-20): (5-15).
[0013] Preferably, the unsaturated organic acid ester monomer is prepared by the following steps: using glycol ether monomers and unsaturated carboxylic acid monomers as raw materials, using hydroquinone as an inhibitor, and reacting at 105-130° C. for 3-6 hours under the catalysis of concentrated sulfuric acid or benzenesulfonic acid.
[0014] Preferably, the molar ratio of the glycol ether monomer to the unsaturated carboxylic acid monomer is 1:1.05-1.50. Such a ratio is conducive to the full reaction of the glycol ether.
[0015] Preferably, the glycol ether monomer is one of ethylene glycol methyl ether, ethylene glycol ethyl ether, ethylene glycol butyl ether, or a combination of two or more thereof; and the unsaturated carboxylic acid monomer is one of acrylic acid, methacrylic acid, fumaric acid, and itaconic acid, or a combination of two or more thereof.
[0016] Preferably, the unsaturated organic acid hydroxy ester is one or a combination of two or more of hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxypropyl methacrylate and hydroxyethyl methacrylate.
[0017] Preferably, the unsaturated terminal polyoxyethylene ether monomer is one or a combination of two or more of methyl allyl polyoxyethylene ether, isobutylene alcohol polyoxyethylene ether, isopentenol polyoxyethylene ether, vinyl polyoxyethylene ether, and hydroxybutyl vinyl polyoxyethylene ether.
[0018] Preferably, the unsaturated amide monomer is any one of acrylamide, methacrylamide, N-hydroxymethyl acrylamide and N-isopropyl acrylamide.
[0019] Preferably, the unsaturated sulfonic acid or its salt is 2-acrylamide-2-methylpropanesulfonic acid, sodium methyl propenesulfonate, sodium allyl sulfonate or sodium p-styrenesulfonate.
[0020] Preferably, the unsaturated acid monomer is one or a combination of two or more of unsaturated acids such as acrylic acid, methacrylic acid, fumaric acid and itaconic acid.
[0021] The second aspect of the present invention provides a method for synthesizing the above-mentioned polycarboxylic acid high-performance water reducer, comprising the following steps:
[0022] S1. According to the raw material composition of the water-retaining block, unsaturated organic acid ester monomers, unsaturated acid monomers, unsaturated amide monomers and unsaturated sulfonic acid or its salt monomers are weighed; then all the unsaturated organic acid ester monomers, unsaturated amide monomers, unsaturated sulfonic acid or its salt monomers and 80-90% of the unsaturated acid monomers are added into deionized water to prepare a mixed monomer A solution;
[0023] S2, according to the raw material composition of the water-reducing block, weigh unsaturated terminal polyoxyethylene ether monomer, unsaturated acid monomer, unsaturated organic acid hydroxy ester monomer; then add all the unsaturated terminal polyoxyethylene ether monomer, unsaturated organic acid hydroxy ester monomer and 80-90% of the unsaturated acid monomer into deionized water to prepare a mixed monomer B solution;
[0024] S3, adding a reducing initiator into deionized water to prepare a reducing initiator C solution;
[0025] S4, adding the remaining 10-20% of the unsaturated acid monomer in step S1, the remaining 10-20% of the unsaturated acid monomer in step S2 and an oxidative initiator into deionized water to prepare a reaction base solution;
[0026] S5, placing the reaction base liquid in a reaction kettle, heating it to 40-60° C., then adding 50% of the mixed monomer A solution and 20% of the reducing initiator C solution into the reaction kettle within 10-40 minutes to carry out a polymerization reaction to obtain a prepolymer with water-retaining properties;
[0027] S6, adding 50% of the mixed monomer B solution and 20% of the reducing initiator C solution to the prepolymer with water-retaining properties within 10-40 minutes, and continuing the reaction to generate a water-reducing block on the obtained prepolymer with water-retaining properties to obtain a block prepolymer I;
[0028] S7, adding 50% of the mixed monomer A solution and 20% of the reducing initiator C solution to the block prepolymer I within 10-40 minutes, and continuing the reaction to generate a water-retaining block on the obtained block prepolymer I to obtain a block prepolymer II;
[0029] S8, adding 25% of the mixed monomer B solution and 20% of the reducing initiator C solution to the block prepolymer II within 10-40 minutes, and continuing the reaction to further generate a water-reducing block on the obtained block prepolymer II to obtain a block prepolymer III;
[0030] S9. Add 20% reducing initiator C solution to the block prepolymer III within 10-40 minutes, and add a chain transfer agent, and continue the reaction until the materials in the kettle react completely to obtain a polycarboxylic acid high-performance water reducer.
[0031] Preferably, in step S3, the amount of the reductive initiator is 0.1% to 1.0% of the total amount of the unsaturated terminal polyoxyethylene ether monomer and the unsaturated acid;
[0032] Preferably, in step S4, the reducing initiator is ascorbic acid; the amount of the oxidizing initiator is 0.1% to 2.0% of the total amount of the unsaturated terminal polyoxyethylene ether monomer and the unsaturated acid, and the oxidizing initiator is hydrogen peroxide.
[0033] Preferably, in step S1, the amount of deionized water is 50-80% of the total amount of the unsaturated organic acid ester monomer, unsaturated amide monomer, unsaturated sulfonic acid or its salt and unsaturated acid monomer used to prepare the mixed monomer A solution.
[0034] Preferably, in step S2, the amount of deionized water used is 50-80% of the total amount of the unsaturated terminal polyoxyethylene ether macromonomer, unsaturated acid monomer, and unsaturated organic acid hydroxy ester monomer used to prepare the mixed monomer B solution.
[0035] The present invention has the following beneficial effects:
[0036] The present invention synthesizes an environmentally friendly, excellent-performance polycarboxylic acid high-performance water-reducing agent with water-retaining properties, and the specific performances are as follows:
[0037] 1. The polycarboxylic acid high-performance water-reducing agent synthesized in the present invention plays an obvious role in the concrete mixture of sand and gravel with poor gradation and quality, and can improve the workability of the concrete mixture, increase the cohesion of the concrete mixture, and has no bleeding and segregation.
[0038] 2. The polycarboxylic acid high-performance water-reducing agent synthesized in the present invention plays an obvious role in the concrete mixture of sand and gravel with high mud content. The slump and expansion of the concrete mixture meet the requirements and the loss over time is small, and the working condition of the mixture is good.
[0039] 3. When the C3A content in cement is low, the alkali content is low, the admixture content is large, the inert material is large, and the cement setting time is long, the polycarboxylic acid high-performance water-reducing agent synthesized by the present invention plays an obvious role in the concrete mixture, avoiding the occurrence of bleeding and delayed bleeding, and the mixture is in good working condition.
[0040] 4. The polycarboxylic acid high-performance water-reducing agent synthesized in the present invention has good adaptability and good dosage flexibility, and can ensure the workability of concrete mixtures and the quality of concrete. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0042] Figure 1 Schematic diagram of the process for synthesizing polycarboxylic acid high performance water reducing agent in Example 1. DETAILED DESCRIPTION
[0043] In the following description, for the purpose of illustration rather than limitation, specific details such as specific system structures and technologies are provided to provide a thorough understanding of the embodiments of the present invention. However, it should be clear to those skilled in the art that the present invention may also be implemented in other embodiments without these specific details.
[0044] Example 1
[0045] Reference Figure 1 , a method for synthesizing a polycarboxylic acid high-performance water-reducing agent, comprising the following steps:
[0046] (1) preparing butyl glycol ether acrylate, specifically comprising the following steps: using butyl glycol ether and acrylic acid as monomer raw materials, wherein the molar ratio of butyl glycol ether to acrylic acid is 1:1.20, using concentrated sulfuric acid accounting for 0.8% of the total mass of the monomer raw materials (the sum of the mass of butyl glycol ether and acrylic acid) as a catalyst, and using hydroquinone accounting for 0.5% of the total mass of the monomer raw materials (the sum of the mass of butyl glycol ether and acrylic acid) as a polymerization inhibitor, reacting at 120° C. for 5 hours to obtain butyl glycol ether acrylate;
[0047] (2) according to the raw material composition of the water-retaining block, ethylene glycol butyl ether acrylate, acrylic acid, acrylamide and sodium allyl sulfonate are weighed in a mass ratio of 35:25:32:8, and then all of the ethylene glycol butyl ether acrylate, acrylamide, sodium allyl sulfonate and 85% of acrylic acid are added to deionized water accounting for 50% of the total mass of the monomers (the sum of the mass of ethylene glycol butyl ether acrylate, acrylic acid, acrylamide and sodium allyl sulfonate), mixed, and prepared a mixed monomer A solution;
[0048] (3) according to the raw material composition of the water-reducing block, methyl allyl polyoxyethylene ether, acrylic acid, and hydroxyethyl acrylate are weighed in a mass ratio of 100:10:12, and then all of the methyl allyl polyoxyethylene ether, hydroxyethyl acrylate, and 85% of acrylic acid are added to deionized water accounting for 50% of the total mass of the monomers (the sum of the mass of methyl allyl polyoxyethylene ether, acrylic acid, and hydroxyethyl acrylate), and mixed to prepare a mixed monomer B solution;
[0049] (4) Weighing 0.6% of the total weight of allyl polyoxyethylene ether and acrylic acid and ascorbic acid, and adding them into deionized water to prepare a 3% mass concentration reductive initiator C solution;
[0050] (5) weighing the remaining 15% of the acrylic acid in step (2), the remaining 15% of the acrylic acid in step (3), and 1.0% of hydrogen peroxide in the total weight of methyl allyl polyoxyethylene ether and acrylic acid, and adding them to deionized water to prepare a reaction base solution;
[0051] (6) placing the reaction base liquid in a reaction kettle, raising the temperature to 40° C., adding 50% by weight of the mixed monomer A solution and 20% by weight of the reducing initiator C solution into the reaction kettle within 0.5 h, and performing a polymerization reaction to obtain a prepolymer having water-retaining properties;
[0052] (7) within 0.5 h, adding 50% by weight of the mixed monomer B solution and 20% by weight of the reducing initiator C solution to the prepolymer I obtained above, and continuing the reaction to generate a water-reducing block on the obtained prepolymer having water-retaining properties, thereby obtaining a block prepolymer I;
[0053] (8) within 0.5 h, adding 50% by weight of the mixed monomer A solution and 20% by weight of the reducing initiator C solution to the block prepolymer I, and continuing the reaction to form a water-retaining block on the obtained block prepolymer I, thereby obtaining a block prepolymer II;
[0054] (9) within 0.5 h, adding 25% by weight of the mixed monomer B solution and 20% by weight of the reducing initiator C solution to the block prepolymer II, and continuing the reaction to further generate a water-reducing block on the obtained block prepolymer II to obtain a block prepolymer III;
[0055] (10) Within 0.5 h, 20% of the total mass of the reducing initiator C solution is added to the block prepolymer III, and a chain transfer agent is added, and the reaction is continued until the materials in the kettle react completely. After keeping warm for 0.5 h, alkali is added for neutralization to obtain a mother liquor of a block polycarboxylic acid high-performance water-reducing agent having water-retaining and water-reducing properties, and an appropriate amount of water is added to adjust the solid content of the polycarboxylic acid high-performance water-reducing agent mother liquor to about 40%.
[0056] Example 2
[0057] (1) preparing an ester of an unsaturated organic acid, specifically ethylene glycol ethyl ether methacrylate, the steps are: using ethylene glycol ethyl ether and acrylic acid as monomer raw materials, wherein the molar ratio of ethylene glycol ethyl ether to acrylic acid is 1:1.50, using concentrated sulfuric acid accounting for 1.0% of the total mass of the monomer raw material (the sum of the mass of ethylene glycol butyl ether and acrylic acid) as a catalyst, and using hydroquinone accounting for 0.6% of the total mass of the monomer raw material as a polymerization inhibitor, reacting at 130° C. for 4 hours to obtain ethylene glycol ethyl ether methacrylate;
[0058] (2) according to the raw material composition of the water-retaining block, ethylene glycol ethyl ether methacrylate, methacrylic acid, methacrylamide and sodium methacrylic acid sulfonate are weighed in a mass ratio of 33:28:30:9, and then all of the ethylene glycol ethyl ether methacrylate, methacrylamide and sodium methacrylic acid sulfonate and 85% of methacrylic acid are added to deionized water accounting for 50% of the total mass of the monomers (the sum of the mass of ethylene glycol ethyl ether methacrylate, methacrylic acid, methacrylamide and sodium methacrylic acid sulfonate), mixed, and prepared a mixed monomer A solution;
[0059] (3) according to the raw material composition of the water-reducing block, methyl allyl polyoxyethylene ether, acrylic acid, and hydroxyethyl acrylate are weighed in a mass ratio of 100:15:15, and then all of the methyl allyl polyoxyethylene ether, hydroxyethyl acrylate, and 85% of acrylic acid are added to deionized water accounting for 50% of the total mass of the monomers (the sum of the mass of methyl allyl polyoxyethylene ether, acrylic acid, and hydroxyethyl acrylate), and mixed to prepare a mixed monomer B solution;
[0060] (4) Weighing 0.6% of the total weight of allyl polyoxyethylene ether and acrylic acid and ascorbic acid, and adding them into deionized water to prepare a 3% mass concentration reductive initiator C solution;
[0061] (5) weighing the remaining 15% of the acrylic acid in step (2), the remaining 15% of the acrylic acid in step (3), and 1.0% of hydrogen peroxide in the total weight of methyl allyl polyoxyethylene ether and acrylic acid, and adding them to deionized water to prepare a reaction base solution;
[0062] (6)-(9): As in Example 1, a mother solution of a segmented polycarboxylic acid high-performance water-reducing agent having water-retaining and water-reducing properties is obtained, and an appropriate amount of water is added to adjust the mother solution to obtain a polycarboxylic acid high-performance water-reducing agent having a solid content of about 40%.
[0063] Example 3
[0064] (1) preparing an ester of an unsaturated organic acid, specifically ethylene glycol methyl ether methacrylate, comprising the following steps: using ethylene glycol methyl ether and acrylic acid as monomer raw materials, wherein the molar ratio of ethylene glycol methyl ether to acrylic acid is 1:1.05, using concentrated sulfuric acid of 1.0% of the total mass of the monomer raw materials (the sum of the mass of ethylene glycol methyl ether and acrylic acid) as a catalyst, and using hydroquinone of 0.6% of the total mass of the monomer raw materials as a polymerization inhibitor, reacting at 105° C. for 6 hours to obtain ethylene glycol methyl ether methacrylate;
[0065] (2) according to the raw material composition of the water-retaining block, ethylene glycol methyl ether methacrylate, methacrylic acid, methacrylamide and sodium methacrylic acid sulfonate are weighed in a mass ratio of 25:25:40:10, and then all of the ethylene glycol methyl ether methacrylate, methacrylamide and sodium methacrylic acid and 85% of methacrylic acid are added to deionized water accounting for 50% of the total mass of the monomers (the sum of the mass of ethylene glycol methyl ether methacrylate, methacrylic acid, methacrylamide and sodium methacrylic acid) and mixed to prepare a mixed monomer A solution;
[0066] (3) according to the raw material composition of the water-reducing block, methyl allyl polyoxyethylene ether, acrylic acid, and hydroxyethyl acrylate are weighed in a mass ratio of 100:20:10, and then all of the methyl allyl polyoxyethylene ether, hydroxyethyl acrylate, and 85% of acrylic acid are added to deionized water accounting for 50% of the total mass of the monomers (the sum of the mass of methyl allyl polyoxyethylene ether, acrylic acid, and hydroxyethyl acrylate), and mixed to prepare a mixed monomer B solution;
[0067] (4) Weighing 0.6% of the total weight of allyl polyoxyethylene ether and acrylic acid and ascorbic acid, and adding them into deionized water to prepare a 3% mass concentration reductive initiator C solution;
[0068] (5) weighing the remaining 15% of the acrylic acid in step (2), the remaining 15% of the acrylic acid in step (3), and 1.0% of hydrogen peroxide in the total weight of methyl allyl polyoxyethylene ether and acrylic acid, and adding them to deionized water to prepare a reaction base solution;
[0069] (6)-(9): As in Example 1, a mother solution of a segmented polycarboxylic acid high-performance water-reducing agent having water-retaining and water-reducing properties was obtained, and an appropriate amount of water was added to adjust the mother solution to obtain a polycarboxylic acid high-performance water-reducing agent having a solid content of about 46%.
[0070] Comparative Example 1
[0071] A general-purpose polycarboxylate high-performance water reducer available on the market.
[0072] Test methods
[0073] The application effect test of the modified polycarboxylic acid water-reducing agent obtained in the above examples and comparative examples:
[0074] The concrete test is strictly carried out in accordance with GB / T8076-2008 "Concrete Admixtures", and the slump, expansion and time loss of the concrete mixture are tested. The C30 concrete mix ratio is used for testing, and the C30 concrete mix ratio is shown in Table 1 below. The admixture is a compounded polycarboxylic acid high-performance water-reducing agent, and the admixture dosage is 2.2% of the cementitious material. The specific compounding is shown in Table 2 below.
[0075] Table 1. C30 concrete mix ratio (per m 3 Concrete material consumption (kg)
[0076] Serial number Cement Type type cement Fly ash water Machine-made sand Stone Admixtures l conch C30 303 76 179 846 993 3.76 2 Red Lion C30 303 76 179 846 993 3.76
[0077] Table 2. Compounding methods of admixtures
[0078] Serial number Universal water reducing agent mother liquor / g Sodium gluconate / g Example 1 / g Example 2 / g Water / g Total / g No. 1 350 30 — — 620 1000 No. 2 175 30 175 — 620 1000 No.3 175 30 — 150 620 1000
[0079] Test results
[0080] In the above synthesized water retaining agent products No. 1, No. 2 and No. 3, the polycarboxylic acid high-performance water reducing agent synthesized in Example 1-2 can achieve the expected purpose by effective compounding. By compounding water retaining agent 1 and polycarboxylic acid high-performance water reducing agent, water retaining agent 1, water retaining agent 2 and polycarboxylic acid high-performance water reducing agent, and testing their specific effects in concrete mixtures, the test results are shown in Table 3 below.
[0081] Table 3. Concrete test results
[0082]
[0083] In the actual concrete test, the initial state of the concrete of No. 1 and No. 4 showed segregation and bleeding, the cohesion of cement paste and coarse aggregate was very poor, large stones were exposed, and the slump loss was serious after 1 hour. The initial state of the concrete of No. 2 and No. 3 was better, the concrete workability was very good, the cohesion was good, there was no bleeding, the whole aggregate was well wrapped, the slump and expansion loss of the concrete was very small after 1 hour, and the concrete workability was good. The initial state of the concrete of No. 5 and No. 6 was better, there was no bleeding, the overall cohesion of the concrete was good, and the slump and fluidity loss of the concrete was small after 1 hour.
[0084] In summary, when low-strength concrete is prepared with machine-made sand, due to the influence of the concrete base material, especially the gradation of machine-made sand and the influence of sand powder content, the adaptability of ordinary polycarboxylic acid high-performance water-reducing agent to the material cannot achieve the expected purpose, resulting in serious concrete segregation, bleeding and slump loss. After ordinary polycarboxylic acid high-performance water-reducing agent is compounded with the polycarboxylic acid high-performance water-reducing agent of the present invention, the initial state and the state after 1 hour of the concrete mixture are relatively good, the concrete mixture does not have bleeding and segregation, and the cohesiveness and workability of the concrete mixture are greatly improved, and the slump and expansion losses are small.
[0085] In practical applications, the compounding ratio of the common polycarboxylic acid high-performance water-reducing agent and the water-retaining polycarboxylic acid high-performance water-reducing agent of the present invention can be adjusted according to actual conditions.
[0086] The present invention is not limited to the above-mentioned specific implementation modes. Various changes made by ordinary technicians in this field based on the above-mentioned concepts without creative work are all within the protection scope of the present invention.
Claims
1. A polycarboxylic acid high performance water reducing agent, characterized in that: The polycarboxylic acid high-performance water-reducing agent is a block polymer, which is composed of a water-retaining block and a water-reducing block, and the mass ratio of the two is 1-2:2-1; The raw material composition of the water-retaining block includes: unsaturated organic acid ester monomer, unsaturated acid monomer, unsaturated amide monomer, unsaturated sulfonic acid or its salt monomer, with a mass ratio of (10-40): (10-30): (10-40): (5-10); The raw material composition of the water-reducing block includes: unsaturated terminal polyoxyethylene ether monomer, unsaturated acid monomer, unsaturated organic acid hydroxy ester monomer, and the mass ratio is 100: (10-20): (5-15).
2. The polycarboxylic acid high performance water reducing agent according to claim 1, characterized in that: The unsaturated organic acid ester monomer is prepared by the following steps: using glycol ether monomers and unsaturated carboxylic acid monomers as raw materials, using hydroquinone as a polymerization inhibitor, and reacting at 105-130° C. for 3-6 hours under the catalysis of concentrated sulfuric acid or benzenesulfonic acid.
3. The polycarboxylic acid high performance water reducing agent according to claim 2, characterized in that: The molar ratio of the glycol ether monomer to the unsaturated carboxylic acid monomer is 1:(1.05-1.50); the glycol ether monomer is one of ethylene glycol methyl ether, ethylene glycol ethyl ether, and ethylene glycol butyl ether, or a combination of two or more thereof; the unsaturated carboxylic acid monomer is one of acrylic acid, methacrylic acid, fumaric acid, and itaconic acid, or a combination of two or more thereof.
4. The polycarboxylic acid high performance water reducing agent according to claim 1, characterized in that: The unsaturated organic acid hydroxy ester is one or a combination of two or more of hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxypropyl methacrylate, and hydroxyethyl methacrylate; the unsaturated terminal polyoxyethylene ether monomer is one or a combination of two or more of methyl allyl polyoxyethylene ether, isobutylene alcohol polyoxyethylene ether, isopentenol polyoxyethylene ether, vinyl polyoxyethylene ether, and hydroxybutyl vinyl polyoxyethylene ether.
5. The polycarboxylic acid high performance water reducing agent according to claim 1, characterized in that: The unsaturated amide monomer is any one of acrylamide, methacrylamide, N-hydroxymethyl acrylamide and N-isopropyl acrylamide; the unsaturated sulfonic acid or its salt monomer is 2-acrylamide-2-methylpropanesulfonic acid, sodium methacrylic sulfonate, sodium allyl sulfonate or sodium p-styrene sulfonate.
6. The polycarboxylic acid high performance water reducing agent according to claim 1, characterized in that: The unsaturated acid monomer is one or a combination of two or more unsaturated acids such as acrylic acid, methacrylic acid, fumaric acid and itaconic acid.
7. A method for synthesizing the polycarboxylic acid high performance water reducing agent according to any one of claims 1 to 6, characterized in that: The following steps are involved: S1. According to the raw material composition of the water-retaining block, unsaturated organic acid ester monomers, unsaturated acid monomers, unsaturated amide monomers and unsaturated sulfonic acid or its salt monomers are weighed; then all the unsaturated organic acid ester monomers, unsaturated amide monomers, unsaturated sulfonic acid or its salt monomers and 80-90% of the unsaturated acid monomers are added into deionized water to prepare a mixed monomer A solution; S2, according to the raw material composition of the water-reducing block, weigh unsaturated terminal polyoxyethylene ether monomer, unsaturated acid monomer, unsaturated organic acid hydroxy ester monomer; then add all the unsaturated terminal polyoxyethylene ether monomer, unsaturated organic acid hydroxy ester monomer and 80-90% of the unsaturated acid monomer into deionized water to prepare a mixed monomer B solution; S3, adding a reducing initiator into deionized water to prepare a reducing initiator C solution; S4, adding the remaining 10-20% of the unsaturated acid monomer in step S1, the remaining 10-20% of the unsaturated acid monomer in step S2 and an oxidative initiator into deionized water to prepare a reaction base solution; S5, placing the reaction base liquid in a reaction kettle, heating it to 40-60° C., then adding 50% of the mixed monomer A solution and 20% of the reducing initiator C solution into the reaction kettle within 10-40 minutes to carry out a polymerization reaction to obtain a prepolymer with water-retaining properties; S6, adding 50% of the mixed monomer B solution and 20% of the reducing initiator C solution to the prepolymer with water-retaining properties within 10-40 minutes, and continuing the reaction to generate a water-reducing block on the obtained prepolymer with water-retaining properties to obtain a block prepolymer I; S7, adding 50% of the mixed monomer A solution and 20% of the reducing initiator C solution to the block prepolymer I within 10-40 minutes, and continuing the reaction to generate a water-retaining block on the obtained block prepolymer I to obtain a block prepolymer II; S8, adding 25% of the mixed monomer B solution and 20% of the reducing initiator C solution to the block prepolymer II within 10-40 minutes, and continuing the reaction to generate a water-reducing block on the obtained block prepolymer II to obtain a block prepolymer III; S9. Add 20% reducing initiator C solution to the block prepolymer III within 10-40 minutes, and add a chain transfer agent, and continue the reaction until the materials in the kettle react completely to obtain a polycarboxylic acid high-performance water reducer.
8. The method for synthesizing the polycarboxylic acid high performance water reducing agent according to claim 7, characterized in that: In step S3, the amount of the reducing initiator is 0.1% to 1.0% of the total mass of the unsaturated terminal polyoxyethylene ether monomer and the unsaturated acid, and the reducing initiator is ascorbic acid; in step S4, the amount of the oxidizing initiator is 0.1% to 2.0% of the total mass of the unsaturated terminal polyoxyethylene ether monomer and the unsaturated acid, and the oxidizing initiator is hydrogen peroxide.
9. The method for synthesizing the polycarboxylic acid high performance water reducing agent according to claim 7, characterized in that: In step S1, the amount of deionized water used is 50-80% of the total amount of unsaturated organic acid ester monomers, unsaturated amide monomers, unsaturated sulfonic acids or their salts and unsaturated acid monomers used to prepare the mixed monomer A solution; in step S2, the amount of deionized water used is 50-80% of the total amount of unsaturated terminal polyoxyethylene ether macromonomers, unsaturated acid monomers and unsaturated organic acid hydroxy ester monomers used to prepare the mixed monomer B solution.
Citation Information
Cited By
Bio-based block copolymer water reducing agent and preparation method thereof
CN121537582A