Method for catalytically synthesizing polyester polyol with low polymerization degree by taking dimethyl oxalate as raw material

By controlling the catalyst and reaction process, dimethyl oxalate reacts with small molecule polyols to synthesize low-polymerization-degree polyester polyols with high ester group content, which solves the shortcomings of existing technologies in improving the performance of polyurethane materials and realizes the improvement of polyurethane material performance.

CN118909232AInactive Publication Date: 2024-11-08INST OF COAL CHEM CHINESE ACAD OF SCI
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411115717.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing technologies have not reported the synthesis of low-polymerization-degree polyester polyols from dimethyl oxalate and their application in the field of polyurethane materials, resulting in insufficient performance improvement of polyurethane materials.

Method used

By controlling the catalyst and reaction process conditions, dimethyl oxalate and small organic molecule polyols are synthesized into low-polymerization degree polyester polyols with higher ester group content through transesterification and compression reduction polymerization, which can be used to prepare polyurethane materials.

Benefits of technology

This improves the intermolecular hydrogen bonding and polarity of polyurethane materials, thereby enhancing their mechanical properties and making them suitable for various applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004993562250000031
    Figure BDA0004993562250000031
Patent Text Reader

Abstract

The invention belongs to the technical field of polyurethane materials, and particularly relates to a method for catalytically synthesizing low-polymerization-degree polyester polyol by taking dimethyl oxalate as a raw material. Dimethyl oxalate is an intermediate product in a coal-to-ethylene glycol process, and has the unique structural characteristics of low cost, easiness in obtaining and high content of ester functional groups in molecules. The novel polyester polyol (the molecular weight is 1000-3000) with high ester group content is synthesized by taking dimethyl oxalate as a raw material through a vacuum melt polymerization method (ester exchange and reduced pressure polycondensation reaction processes), and the novel polyester polyol can be used for preparing polyurethane materials, is expected to endow the polyurethane materials with stronger polarity and intermolecular hydrogen-bond interaction, and improves the mechanical properties of the materials. The method disclosed by the invention not only meets the national strategic requirement on high-efficiency and low-carbon utilization of coal, but also meets the concept of green chemical development, and meanwhile, has great commercial value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polyurethane materials, and particularly relates to a method for catalytically synthesizing low-polymerization degree polyester polyols by taking dimethyl oxalate as a raw material. Background Art

[0002] Polyurethane (PU) is a class of polymer materials with excellent performance, usually prepared by polymerization reaction with polyol, polyisocyanate and chain extender as main raw materials. Because PU molecular structure contains repeated rigid urethane segments (hard segments) and flexible polyol segments, it has excellent mechanical properties, wear resistance, flexibility, weather resistance, chemical resistance, processing performance and performance adjustability. It can be made into elastomers, foams, fibers, synthetic leather, coatings and adhesives, etc., and is widely used in various fields of social production and life such as aerospace, construction and building materials, transportation, textile machinery, sports equipment, clothing and footwear, electricity, mining, etc. With the continuous expansion of the application scope of polyurethane, the requirements for polyurethane performance are gradually increasing. Developing new polyurethane raw materials and improving the performance of polyurethane materials to meet different application requirements have become an important direction of polyurethane development in recent years.

[0003] Polyester polyols are one of the important raw materials for synthesizing polyurethane materials, and are mainly used to synthesize high-performance polyurethane elastomers. The synthesis of polyester polyols is usually prepared by vacuum melt polymerization (ester exchange and reduced pressure polyurethane reaction process) using dimethyl dicarboxylate and small molecule polyols as raw materials. Since polyester polyols contain highly polar ester functional groups, the hydrogen bonding effect in the prepared polyurethane material is significantly improved, making the material have better mechanical properties, thermal stability, oil resistance, etc. Compared with polyether polyols, polyester polyols have a wider range of molecular structure design and adjustment due to the rich types of small molecule polyols and organic carboxylic acid dimethyl esters, and there are more types of related polyurethane products.

[0004] Dimethyl oxalate (DMO) is an important organic reaction monomer with the smallest molecular weight, the highest ester content, the strongest molecular polarity and the strongest intermolecular hydrogen bonding force among organic dicarboxylic acid diesters. It is widely used in organic synthesis and drug synthesis. Moreover, DMO can be widely and cheaply obtained from the industrial catalytic hydrogenation of coal-based synthesis gas (CO and H2 mixed gas) to prepare ethylene glycol. For example, patent CN115490838A discloses a method for preparing a high molecular weight (average molecular weight: 60,000 to 100,000) aliphatic polyoxalate, which can significantly increase the molecular weight of aliphatic polyoxalate polymers and reduce the molecular weight distribution. The obtained aliphatic polyoxalate products have high strength, toughness and good hue, and can be directly used as degradable plastic masterbatch. For example, patent CN115785410A proposes a polyethylene oxalate copolyester and a synthesis method, which uses dimethyl oxalate and ethylene glycol as monomer raw materials, and is prepared by ester exchange reaction, pre-condensation reaction and final condensation reaction in sequence with the addition of a third monomer and a catalyst. The synthesized polyethylene oxalate copolyester has a thermal decomposition 5% temperature of above 240°C, which greatly improves the thermal stability of the homopolymer. Another example is patent CN113527644A, which discloses a method for preparing high molecular weight (average molecular weight: 40,000 to 70,000) polyoxalate hexanediol ester, which uses 1,6-hexanediol and oxalic acid diester to prepare hydroxyl-terminated prepolymer A by transesterification under normal pressure, and uses low-boiling diol and oxalic acid diester to prepare hydroxyl-terminated prepolymer B by transesterification under normal pressure. By adjusting the feed ratio of the two prepolymers A and B, the polyoxalate hexanediol ester described in the invention can be obtained by decompression polymerization at 150°C to 220°C for 0.5hr to 6hr. The product has high molecular weight, excellent color, can be biodegraded and recycled, and is applied to the field of general plastics. At present, only the preparation of high molecular weight degradable and recyclable polyester using dimethyl oxalate as a reaction monomer is reported in patents, while the synthesis of low polymerization degree polyester polyol (average molecular weight: 1000 to 3000) using dimethyl oxalate as a raw material and its application in the field of polyurethane materials has not been reported. Summary of the invention

[0005] The purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art and provide a method for catalytically synthesizing a low-polymerization degree polyester polyol using dimethyl oxalate as a raw material. The present invention synthesizes a novel low-polymerization degree polyester polyol with a higher ester content by ester exchange reaction and reduced pressure polyurethane reaction of dimethyl oxalate and an organic small molecule polyol through the regulation of catalyst and reaction process conditions (reaction formula is as follows), and further applies it to the preparation of polyurethane materials.

[0006]

[0007] (where R represents an alkyl segment with ≥4 C atoms)

[0008] Compared with traditional polyester polyols, due to the introduction of special dimethyl oxalate chain segments, the prepared polyurethane macromolecular segment structure has a higher ester group content and stronger intermolecular hydrogen bonding, which is expected to give polyurethane materials more distinctive properties and provide a new path for the development of new polyurethane products.

[0009] To achieve the above object, the technical solution of the present invention is as follows:

[0010] On the one hand, the present invention provides a method for catalytically synthesizing a low-polymerization degree polyester polyol using dimethyl oxalate as a raw material, comprising the following steps:

[0011] Step 1, transesterification reaction stage: under normal pressure, dimethyl oxalate, a small molecule polyol and a catalyst are mixed, and the temperature is raised to a reaction temperature to carry out a transesterification reaction between dimethyl oxalate and the small molecule polyol;

[0012] Step 2, reduced pressure polyurethane reaction stage: reduce the pressure from normal pressure to high vacuum in stages, and increase the reaction temperature to the set temperature to remove by-products and excess small molecule polyols to achieve the growth of molecular chain segments; after the reaction is completed, cool down to obtain polyester polyols with an average molecular weight of 1000 to 3000.

[0013] Furthermore, in step 1, the small molecule polyol is a straight-chain saturated fatty alcohol, the number of its C atoms is 5 to 10, and the hydroxyl functionality is ≥2; or a branched saturated fatty alcohol, the number of its C atoms is 4 to 10, and the hydroxyl functionality is ≥2.

[0014] Furthermore, the straight-chain saturated fatty alcohol is one or more of 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, dipropylene glycol, triethylene glycol or tetraethylene glycol; the branched-chain saturated fatty alcohol is one or more of 2-methyl-1,3-propanediol, neopentyl glycol, 1,3-butanediol, 2-ethyl-hexanediol, 3-methyl-1,5-pentanediol, 2,4-diethyl-1,5-pentanediol, 2,2,4-trimethyl-1,3-pentanediol, 2-butyl-2-ethyl-1,3-propanediol, 2-ethyl-1,3-hexanediol, 2-methyl-1,8-octanediol or trimethylolpropane.

[0015] Furthermore, the catalyst in step 1 is one of an organic titanate chelate, an organic tin compound, an organic amine compound, a Mg-Al hydrotalcite or a Ca-Zr-Ni based catalyst.

[0016] Furthermore, the organic titanate chelate is one of bis(ethyl acetoacetate) di-n-butoxy titanate chelate, bistriethanolamine diisopropyl titanate chelate, bis(ethyl acetoacetate) diisobutyl titanate chelate, bis(ethyl acetoacetate) diisopropyl titanate chelate, bis(ethyl acetoacetate) diisopropyl titanate chelate, bis(acetylacetonate) ethoxyisopropoxy titanate chelate, bis(acetylacetonate) isobutoxyisopropoxy titanate chelate, and bis(acetylacetonate) diisopropyl titanate chelate.

[0017] Furthermore, the amount of the catalyst in step 1 is 50ppm to 1000ppm of the mass of the small molecule polyol in the ester exchange reaction stage; the molar ratio of dimethyl oxalate to the small molecule polyol is 1:1 to 2; the temperature of the ester exchange reaction is 130 to 230°C, and the time is 4hr to 12hr.

[0018] Furthermore, the amount of the catalyst used is 100ppm to 300ppm of the mass of the small molecule polyol in the ester exchange reaction stage, the molar ratio of dimethyl oxalate to the small molecule polyol is 1:1 to 1.5, and the ester exchange reaction time is 6hr to 8hr.

[0019] Furthermore, in step 2, the pressure is reduced from normal pressure to -0.050 MPa to -0.095 MPa in stages, the temperature of the polycondensation reaction is 160° C. to 250° C., and the time is 2 hr to 12 hr.

[0020] Furthermore, the polycondensation reaction is carried out at a temperature of 180° C. to 210° C. and for a time of 3 hr to 6 hr.

[0021] Another aspect of the present invention provides the use of the low-polymerization degree polyester polyol prepared by the method as described above in the synthesis of polyurethane materials.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] The dimethyl oxalate used in the present invention is an intermediate product of the coal-to-ethylene glycol process, has high purity, stable properties, is cheap and easy to obtain, and in particular, dimethyl oxalate has a unique functional group structure with a high ester content in the molecule, and is an alkyd diester compound with the shortest molecular chain segment. The prepared low-polymerization degree polyester polyol is a polyol of a new structure, and the relevant preparation method has not been reported. This polyester polyol has a higher ester group content, and when used for the synthesis of polyurethane materials, it can give the polyurethane materials stronger polarity and intermolecular hydrogen bonding, and is expected to improve the mechanical properties of the polyurethane materials. DETAILED DESCRIPTION

[0024] In order to facilitate the understanding of the present invention, the present invention will be described more fully below. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.

[0025] Example 1

[0026] A method for catalytically synthesizing low-polymerization degree polyester polyols using dimethyl oxalate as a raw material comprises the following steps:

[0027] Step 1, transesterification reaction stage: In a clean 500mL four-necked flask equipped with a stirring system, a heating system, a temperature measuring system and a distillation column with a top reflux distributor, add 112.84g (1.083mol) of 1,5-pentanediol (1,5-PD, chemically pure, without dehydration treatment), 118.09g (1mol) of dimethyl oxalate (DMO) and 0.01128g (100ppm / wt. raw material small molecule diol) of titanate chelate (bis (acetylacetonato) diisopropyl titanate) catalyst. Open the condensation water at the top of the distillation column, preheat the distillation column (control the wall temperature at about 70°C), purge the air in the reactor with nitrogen, start stirring, and quickly heat the reactor temperature to 138°C. Methanol condensation reflux appears at the top of the distillation column. Open the reflux distributor to remove the methanol generated by the transesterification reaction. The reaction is continued for 6 hours at 138°C to 220°C under normal pressure.

[0028] Step 2, reduced pressure polycondensation stage: In the reduced pressure polycondensation stage, the reaction temperature is controlled at 180°C to 190°C, and the pressure is reduced from normal pressure to -0.05MPa, -0.06MPa, -0.07MPa, -0.08MPa, and -0.095MPa in stages. The reduced pressure polycondensation reaction is continued for 5 hours to remove by-products and excess small molecule alcohols. The target product, low polymerization degree polyester polyol - P(DMO / 1,5-PD)Diol-2000, is obtained by cooling.

[0029] At room temperature, the product P(DMO / 1,5-PD)Diol-2000 is a light yellow liquid with a hydroxyl value of 54.68 mgKOH / g, an acid value of 0.05 mgKOH / g, an average molecular weight of 2050, a yield of 90.02%, and an ester content of 52.76%wt. The product P(DMO / 1,5-PD)Diol-2000 was reacted with diphenylmethane-4,4'-diisocyanate (MDI) to prepare a prepolymer with free-NCO%=8.5%, and the prepolymer was chain extended with a small molecule diol 1,4-butanediol (1,4-BDO) to prepare a polyurethane elastomer sample. The test performance results are: hardness Shore A95, tensile strength 19.2MPa, elongation at break 406.7%, tear strength 91KN / m, and impact rebound rate 19%.

[0030] Example 2

[0031] A method for catalytically synthesizing low-polymerization degree polyester polyols using dimethyl oxalate as a raw material comprises the following steps:

[0032] Step 1, transesterification reaction stage: In a clean 500mL four-necked flask equipped with a stirring system, a heating system, a temperature measuring system and a distillation column with a top reflux distributor, add 141.24g (1.195mol) of 1,6-hexanediol (1,6-HD, industrial grade, not dehydrated), 118.09g (1mol) of dimethyl oxalate (DMO) and 0.01412g (100ppm / wt. raw material small molecule diol) of titanate chelate (bis (acetylacetonato) diisopropyl titanate) catalyst. Open the condensation water at the top of the distillation column, preheat the distillation column (control the wall temperature at about 70°C), purge the air in the reactor with nitrogen, start stirring, and quickly heat the reactor temperature to 139°C. Methanol condensation reflux appears at the top of the distillation column. Open the reflux distributor to remove the methanol generated by the transesterification reaction. The reaction is continued for 6 hours at 139°C to 220°C under normal pressure.

[0033] Step 2, reduced pressure polyurethane stage: In the reduced pressure polyurethane stage, the reaction temperature is controlled at 180°C to 190°C, and the pressure is reduced from normal pressure to -0.05MPa, -0.06MPa, -0.07MPa, -0.08MPa, and -0.095MPa in stages. The reduced pressure polyurethane reaction is continued for 4 hours to remove by-products and excess small molecule alcohols. The target product, low polymerization degree polyester polyol - P(DMO / 1,6-HD)Diol-1000, is obtained by cooling.

[0034] At room temperature, the product P(DMO / 1,6-HD)Diol-1000 is a light yellow solid with a hydroxyl value of 102.58 mgKOH / g, an acid value of 0.05 mgKOH / g, an average molecular weight of 1093.29, a yield of 96.18%, and an ester content of 45.08%wt. The product P(DMO / 1,6HD)Diol-1000 was reacted with diphenylmethane-4,4'-diisocyanate (MDI) to prepare a prepolymer with free-NCO%=8.5%, and the prepolymer was chain extended with a small molecule diol 1,4-butanediol (1,4-BDO) to prepare a polyurethane elastomer sample. The test performance results are: hardness Shao A97, tensile strength 39.8MPa, elongation at break 458.2%, tear strength 163.5KN / m, and impact rebound rate 19%.

[0035] Example 3

[0036] A method for catalytically synthesizing low-polymerization degree polyester polyols using dimethyl oxalate as a raw material comprises the following steps:

[0037] Step 1, transesterification reaction stage: In a clean 500mL four-necked flask equipped with a stirring system, a heating system, a temperature measuring system and a distillation column with a top reflux distributor, add 128.98g (1.092mol) of 1,6-hexanediol (1,6-HD, industrial grade, not dehydrated), 118.09g (1mol) of dimethyl oxalate (DMO) and 0.01290g (100ppm / wt. raw material small molecule diol) of titanate chelate (bis (acetylacetonato) diisopropyl titanate) catalyst. Open the condensation water at the top of the distillation column, preheat the distillation column (control the wall temperature at about 70°C), purge the air in the reactor with nitrogen, start stirring, and quickly heat the reactor temperature to 139°C. Methanol condensation reflux appears at the top of the distillation column. Open the reflux distributor to remove the methanol generated by the transesterification reaction. The reaction is continued for 6 hours at 139°C to 220°C under normal pressure.

[0038] Step 2, reduced pressure polycondensation stage: In the reduced pressure polycondensation stage, the reaction temperature is controlled at 180°C to 200°C, and the pressure is reduced from normal pressure to -0.05MPa, -0.06MPa, -0.07MPa, -0.08MPa, and -0.095MPa in stages. The reduced pressure polycondensation reaction is continued for 5 hours to remove by-products and excess small molecule alcohols. The target product, low polymerization degree polyester polyol - P(DMO / 1,6-HD)Diol-2000, is obtained by cooling.

[0039] At room temperature, the product P(DMO / 1,6-HD)Diol-2000 is a light yellow solid with a hydroxyl value of 53.98 mgKOH / g, an acid value of 0.05 mgKOH / g, an average molecular weight of 2076.62, a yield of 95.25%, and an ester content of 48.10%wt. The product P(DMO / 1,6-HD)Diol-2000 was reacted with diphenylmethane-4,4'-diisocyanate (MDI) to prepare a prepolymer with free-NCO%=8.5%, and the prepolymer was chain extended with a small molecule diol 1,4-butanediol (1,4-BDO) to prepare a polyurethane elastomer sample. The test performance results are: hardness Shore A96, tensile strength 35.6MPa, elongation at break 497.3%, tear strength 159.6KN / m, and impact rebound rate 20%.

[0040] Example 4

[0041] A method for catalytically synthesizing low-polymerization degree polyester polyols using dimethyl oxalate as a raw material comprises the following steps:

[0042] Step 1, transesterification reaction stage: In a clean 500mL four-necked flask equipped with a stirring system, a heating system, a temperature measuring system and a distillation column with a top reflux distributor, add 125.14g (1.060mol) of 1,6-hexanediol (1,6-HD, industrial grade, not dehydrated), 118.09g (1mol) of dimethyl oxalate (DMO) and 0.01251g (100ppm / wt. raw material small molecule diol) of titanate chelate (bis (acetylacetonato) diisopropyl titanate) catalyst. Open the condensation water at the top of the distillation column, preheat the distillation column (control the wall temperature at about 70°C), purge the air in the reactor with nitrogen, start stirring, and quickly heat the reactor temperature to 139°C. Methanol condensation reflux appears at the top of the distillation column. Open the reflux distributor to remove the methanol generated by the transesterification reaction. The reaction is continued for 6 hours at 139°C to 220°C under normal pressure.

[0043] Step 2, reduced pressure polycondensation stage: In the reduced pressure polycondensation stage, the reaction temperature is controlled at 180°C to 210°C, and the pressure is reduced from normal pressure to -0.05MPa, -0.06MPa, -0.07MPa, -0.08MPa, and -0.095MPa in stages. The reduced pressure polycondensation reaction is continued for 6 hours to remove by-products and excess small molecule alcohols. The target product, low polymerization degree polyester polyol - P(DMO / 1,6-HD)Diol-3000, is obtained by cooling.

[0044] At room temperature, the product P(DMO / 1,6-HD)Diol-3000 is a light yellow solid with a hydroxyl value of 35.84 mgKOH / g, an acid value of 0.05 mgKOH / g, an average molecular weight of 3126.17, a yield of 94.63%, and an ester content of 49.11%wt. The product P(DMO / 1,6-HD)Diol-3000 was reacted with diphenylmethane-4,4'-diisocyanate (MDI) to prepare a prepolymer with free-NCO%=8.5%, and the prepolymer was chain extended with a small molecule diol 1,4-butanediol (1,4-BDO) to prepare a polyurethane elastomer sample. The test performance results are: hardness Shore A94, tensile strength 34.8MPa, elongation at break 516.2%, tear strength 158.2KN / m, and impact rebound rate 22%.

[0045] Example 5

[0046] A method for catalytically synthesizing low-polymerization degree polyester polyols using dimethyl oxalate as a raw material comprises the following steps:

[0047] Step 1, transesterification reaction stage: In a clean 500mL four-necked flask equipped with a stirring system, a heating system, a temperature measuring system and a distillation column with a top reflux distributor, 128.98g (1.092mol) of 1,6-hexanediol (1,6-HD, industrial grade, not dehydrated), 118.09g (1mol) of dimethyl oxalate (DMO), 0.00645g (50ppm / wt. raw material small molecule diol) of titanate chelate (bis(acetylacetonate) diisopropyl titanate) catalyst and 0.00645g (50ppm / wt. raw material small molecule diol) of titanate chelate (bis(ethyl acetoacetate) diisopropyl titanate) catalyst were added. Start condensing water on the top of the distillation column, preheat the distillation column (control the wall temperature at about 70°C), purge the air in the reactor with nitrogen, start stirring, quickly heat the reactor temperature to 138°C, condense and reflux methanol at the top of the distillation column, open the reflux distributor to remove the methanol generated by the ester exchange reaction, and continue the reaction for 6 hours in the range of 138°C to 220°C at normal pressure.

[0048] Step 2, reduced pressure polycondensation stage: In the reduced pressure polycondensation stage, the reaction temperature is controlled at 180°C to 200°C, and the pressure is reduced from normal pressure to -0.05MPa, -0.06MPa, -0.07MPa, -0.08MPa, and -0.095MPa in stages. The reduced pressure polycondensation reaction is continued for 5 hours to remove by-products and excess small molecule alcohols. The target product, low polymerization degree polyester polyol - P(DMO / 1,6-HD)Diol-2000, is obtained by cooling.

[0049] At room temperature, the product P(DMO / 1,6-HD)Diol-2000 is a light yellow solid with a hydroxyl value of 52.97 mgKOH / g, an acid value of 0.05 mgKOH / g, an average molecular weight of 2116.29, a yield of 95.39%, and an ester content of 48.10%wt. The product P(DMO / 1,6-HD)Diol-2000 was reacted with diphenylmethane-4,4'-diisocyanate (MDI) to prepare a prepolymer with free-NCO%=8.5%, and the prepolymer was chain extended with a small molecule diol 1,4-butanediol (1,4-BDO) to prepare a polyurethane elastomer sample. The test performance results are: hardness Shore A96, tensile strength 35.3MPa, elongation at break 495.8%, tear strength 158.7KN / m, and impact rebound rate 20%.

[0050] Example 6

[0051] A method for catalytically synthesizing low-polymerization degree polyester polyols using dimethyl oxalate as a raw material comprises the following steps:

[0052] Step 1, transesterification reaction stage: In a clean 500mL four-necked flask equipped with a stirring system, a heating system, a temperature measuring system and a distillation column with a top reflux distributor, add 145.38g (1.0997mol) of 1,7-heptanediol (1,7-HPD, chemically pure, without dehydration treatment), 118.09g (1mol) of dimethyl oxalate (DMO) and 0.02908g (200ppm / wt. raw material small molecule diol) of titanate chelate (bis (ethyl acetoacetate) di-n-butoxy titanate) catalyst. Open the condensation water at the top of the distillation column, preheat the distillation column (control the wall temperature at about 70°C), purge the air in the reactor with nitrogen, start stirring, and quickly heat the reactor temperature to 141°C. Methanol condensation reflux appears at the top of the distillation column. Open the reflux distributor to remove the methanol generated by the transesterification reaction. The reaction is continued for 6 hours at 141°C to 220°C under normal pressure.

[0053] Step 2, reduced pressure polycondensation stage: In the reduced pressure polycondensation stage, the reaction temperature is controlled at 180°C to 200°C, and the pressure is reduced from normal pressure to -0.05MPa, -0.06MPa, -0.07MPa, -0.08MPa, and -0.095MPa in stages, and the reduced pressure polycondensation reaction is continuously carried out for 5.5 hours to remove by-products and excess small molecule alcohols. The target product, low polymerization degree polyester polyol - P(DMO / 1,7-HPD)Diol-2000, is obtained by cooling.

[0054] At room temperature, the product P(DMO / 1,7-HPD)Diol-2000 is a light yellow solid with a hydroxyl value of 53.98 mgKOH / g, an acid value of 0.05 mgKOH / g, an average molecular weight of 2051.87, a yield of 96.68%, and an ester content of 44.15%wt. The product P(DMO / 1,7-HPD)Diol-2000 was reacted with diphenylmethane-4,4'-diisocyanate (MDI) to prepare a prepolymer with free-NCO%=8.5%, and the prepolymer was chain extended with a small molecule diol 1,4-butanediol (1,4-BDO) to prepare a polyurethane elastomer sample. The test performance results are: hardness Shao A95, tensile strength 32.7MPa, elongation at break 541.8%, tear strength 146.5KN / m, and impact rebound rate 19%.

[0055] Example 7

[0056] A method for catalytically synthesizing low-polymerization degree polyester polyols using dimethyl oxalate as a raw material comprises the following steps:

[0057] Step 1, transesterification reaction stage: In a clean 500mL four-necked flask equipped with a stirring system, a heating system, a temperature measuring system and a distillation column with a top reflux distributor, add 162.03g (1.10802mol) of 1,8-octanediol (1,8-OCD, chemically pure, without dehydration treatment), 118.09g (1mol) of dimethyl oxalate (DMO) and 0.03241g (200ppm / wt. raw material small molecule diol) of titanate chelate (bistriethanolamine diisopropyl titanate) catalyst. Open the condensation water at the top of the distillation column, preheat the distillation column (control the wall temperature at about 70°C), purge the air in the reactor with nitrogen, start stirring, quickly heat the reactor temperature to 150°C, methanol condensation reflux appears at the top of the distillation column, open the reflux distributor to remove the methanol generated by the transesterification reaction, and react continuously for 6 hours in the range of 150°C to 225°C at normal pressure.

[0058] Step 2, reduced pressure polycondensation stage: In the reduced pressure polycondensation stage, the reaction temperature is controlled at 180°C to 200°C, and the pressure is reduced from normal pressure to -0.05MPa, -0.06MPa, -0.07MPa, -0.08MPa, and -0.095MPa in stages, and the reduced pressure polycondensation reaction is continuously carried out for 5.5 hours to remove by-products and excess small molecule alcohols. The target product, low polymerization degree polyester polyol - P(DMO / 1,8-OCD)Diol-2000, is obtained by cooling.

[0059] At room temperature, the product P(DMO / 1,8-OCD)Diol-2000 is a light yellow solid with a hydroxyl value of 52.97 mgKOH / g, an acid value of 0.05 mgKOH / g, an average molecular weight of 2116.31, a yield of 97.59%, and an ester content of 40.74%wt. The product P(DMO / 1,8-OCD)Diol-2000 was reacted with diphenylmethane-4,4'-diisocyanate (MDI) to prepare a prepolymer with free-NCO%=8.5%, and the prepolymer was chain extended with a small molecule diol 1,4-butanediol (1,4-BDO) to prepare a polyurethane elastomer sample. The test performance results are: hardness Shore A95, tensile strength 30.2MPa, elongation at break 599.3%, tear strength 135.2KN / m, and impact rebound rate 18%.

[0060] Example 8

[0061] A method for catalytically synthesizing low-polymerization degree polyester polyols using dimethyl oxalate as a raw material comprises the following steps:

[0062] Step 1, transesterification reaction stage: In a clean 500mL four-necked flask equipped with a stirring system, a heating system, a temperature measuring system and a distillation column with a top reflux distributor, add 196.07g (1.12504mol) of 1,10-decanediol (1,10-DD, chemically pure, not dehydrated), 118.09g (1mol) of dimethyl oxalate (DMO) and 0.03921g (200ppm / wt. raw material small molecule diol) of titanate chelate (bis (ethyl acetoacetate) titanate diisopropyl ester) catalyst. Open the condensation water at the top of the distillation column, preheat the distillation column (control the wall temperature at about 70°C), purge the air in the reactor with nitrogen, start stirring, and quickly heat the reactor temperature to 155°C. Methanol condensation reflux appears at the top of the distillation column. Open the reflux distributor to remove the methanol generated by the transesterification reaction. The reaction is continued for 6 hours at 155°C to 225°C under normal pressure.

[0063] Step 2, reduced pressure polycondensation stage: In the reduced pressure polycondensation stage, the reaction temperature is controlled at 180°C to 200°C, and the pressure is reduced from normal pressure to -0.05MPa, -0.06MPa, -0.07MPa, -0.08MPa, and -0.095MPa in stages. The reduced pressure polycondensation reaction is continued for 6 hours to remove by-products and excess small molecule alcohols. The target product, low polymerization degree polyester polyol - P(DMO / 1,10-DD)Diol-2000, is obtained by cooling.

[0064] At room temperature, the product P(DMO / 1,10-DD)Diol-2000 is a light yellow solid with a hydroxyl value of 54.82 mgKOH / g, an acid value of 0.05 mgKOH / g, an average molecular weight of 2044.69, a yield of 98.72%, and an ester content of 35.20%wt. The product P(DMO / 1,10-DD)Diol-2000 was reacted with diphenylmethane-4,4'-diisocyanate (MDI) to prepare a prepolymer with free-NCO%=8.5%, and the prepolymer was chain extended with a small molecule diol 1,4-butanediol (1,4-BDO) to prepare a polyurethane elastomer sample. The test performance results are: hardness Shore A93, tensile strength 26.1 MPa, elongation at break 715.3%, tear strength 116.8 KN / m, and impact rebound rate 16%.

[0065] Example 9

[0066] A method for catalytically synthesizing low-polymerization degree polyester polyols using dimethyl oxalate as a raw material comprises the following steps:

[0067] Step 1, transesterification reaction stage: In a clean 500mL four-necked flask equipped with a stirring system, a heating system, a temperature measuring system and a distillation column with a tower top reflux distributor, 186.25g (1.2403mol) of triethylene glycol (TEG, purity: 98%, not dehydrated), 118.09g (1mol) of dimethyl oxalate (DMO) and 0.05016g (269.3ppm / wt. raw material small molecule diol) of titanate chelate (bis (acetylacetonato) ethoxyisopropoxy titanate) catalyst were added. The distillation column top was opened to condense water, the distillation column was preheated (the wall temperature was controlled at about 70°C), nitrogen was purged to replace the air in the reactor, stirring was started, and the reactor temperature was quickly heated to 135°C. Methanol condensation reflux appeared at the top of the distillation column, and the reflux distributor was opened to remove the methanol generated by the transesterification reaction. The reaction was continued for 6 hours in the range of 135°C to 222°C under normal pressure.

[0068] Step 2, reduced pressure polycondensation stage: In the reduced pressure polycondensation stage, the reaction temperature is controlled at 180°C to 190°C, and the pressure is reduced from normal pressure to -0.05MPa, -0.06MPa, -0.07MPa, -0.08MPa, and -0.095MPa in stages. The reduced pressure polycondensation reaction is continued for 4 hours to remove by-products and excess small molecule alcohols. The target product, low polymerization degree polyester polyol - P(DMO / TEG)Diol-1000, is obtained by cooling.

[0069] At room temperature, the product P(DMO / TEG)Diol-1000 is a light yellow liquid with a hydroxyl value of 99.15 mgKOH / g, an acid value of 0.05 mgKOH / g, an average molecular weight of 1131, a yield of 87.45%, and an ester content of 36.63%wt. The product P(DMO / TEG)Diol-1000 is reacted with diphenylmethane-4,4'-diisocyanate (MDI) to prepare a prepolymer with free-NCO%=8.5%, and a polyurethane elastomer sample is prepared by chain extension with a small molecule diol 1,4-butanediol (1,4-BDO). The test performance results are: hardness Shore A97, tensile strength 31.30 MPa, elongation at break 620.3%, tear strength 142.5 KN / m, and impact rebound rate 15%.

[0070] Example 10

[0071] A method for catalytically synthesizing low-polymerization degree polyester polyols using dimethyl oxalate as a raw material comprises the following steps:

[0072] Step 1, transesterification reaction stage: In a clean 500mL four-necked flask equipped with a stirring system, a heating system, a temperature measuring system and a distillation column with a tower top reflux distributor, 30g (0.2408mol) of triethylene glycol (TEG, purity: 98%, not dehydrated), 119.98g (0.9632mol) of 1,6-hexanediol (1,6-HD, industrial grade, not dehydrated), 118.09g (1mol) of dimethyl oxalate (DMO) and 0.0150g (100ppm / wt. raw material small molecule diol) of titanate chelate (bis(acetylacetonato)isobutoxyisopropoxytitanate) catalyst were added. Start condensing water on the top of the distillation column, preheat the distillation column (control the wall temperature at about 70°C), purge the air in the reactor with nitrogen, start stirring, quickly heat the reactor temperature to 138°C, condense and reflux methanol at the top of the distillation column, open the reflux distributor to remove the methanol generated by the ester exchange reaction, and continue the reaction for 6 hours in the range of 138°C to 227°C at normal pressure.

[0073] Step 2, reduced pressure polymerization stage: In the reduced pressure polymerization stage, the reaction temperature is controlled at 180℃~190℃, and the pressure is reduced from normal pressure to -0.05MPa, -0.06MPa, -0.07MPa, -0.08MPa, -0.095MPa in stages, and the reduced pressure polymerization reaction is continued for 4 hours to remove by-products and excess small molecule alcohols. The target product, low polymerization degree polyester polyol -P﹝DMO / (TEG 0.2 +HD 0.8 )﹞Diol-1000.

[0074] At room temperature, the product P﹝DMO / (TEG 0.2 +HD 0.8 )﹞Diol-1000 is a light yellow liquid with a hydroxyl value of 111.38 mgKOH / g, an acid value of 0.04 mgKOH / g, an average molecular weight of 1007, a yield of 94.38%, and an ester content of 43.15%wt. 0.2 +HD 0.8 )﹞Diol-1000 was reacted with diphenylmethane-4,4'-diisocyanate (MDI) to prepare a prepolymer with free -NCO%=8.5%, which was then chain extended with a small molecule diol 1,4-butanediol (1,4-BDO) to prepare a polyurethane elastomer sample. The test performance results showed: Shore A hardness 95, tensile strength 34.3MPa, elongation at break 583.3%, tear strength 144.7KN / m, and impact rebound rate 17%.

[0075] Embodiment 11

[0076] A method for catalytically synthesizing low-polymerization degree polyester polyols using dimethyl oxalate as a raw material comprises the following steps:

[0077] Step 1, transesterification reaction stage: In a clean 500mL four-necked flask equipped with a stirring system, a heating system, a temperature measuring system and a distillation column with a top reflux distributor, 64.49g (0.54575mol) of 3-methyl-1,5-pentanediol (3-M-1,5-PD, chemically pure, not dehydrated), 64.49g (0.54575mol) of 1,6-hexanediol (1,6-HD, industrial grade, not dehydrated), 118.09g (1mol) of dimethyl oxalate (DMO) and 0.0258g (200ppm / wt. raw material small molecule diol) of titanate chelate (bis(ethyl acetoacetate) diisobutyl titanate) catalyst were added. Start condensing water on the top of the distillation column, preheat the distillation column (control the wall temperature at about 70°C), purge the air in the reactor with nitrogen, start stirring, quickly heat the reactor temperature to 140°C, condense and reflux methanol at the top of the distillation column, open the reflux distributor to remove the methanol generated by the ester exchange reaction, and continue the reaction for 6 hours in the range of 140°C to 220°C at normal pressure.

[0078] Step 2, reduced pressure polymerization stage: In the reduced pressure polymerization stage, the reaction temperature is controlled at 180℃~200℃, and the pressure is reduced from normal pressure to -0.05MPa, -0.06MPa, -0.07MPa, -0.08MPa, -0.095MPa in stages, and the reduced pressure polymerization reaction is continued for 5 hours to remove by-products and excess small molecule alcohols. The target product, low polymerization degree polyester polyol -P﹝DMO / (3-M-1,5-PD 0.5 +HD 0.5 )﹞Diol-2000.

[0079] At room temperature, the product P﹝DMO / (3-M-1,5-PD 0.5 +HD 0.5 )﹞Diol-2000 is a light yellow liquid with a hydroxyl value of 54.28 mgKOH / g, an acid value of 0.05 mgKOH / g, an average molecular weight of 2065, a yield of 97.52%, and an ester content of 48.10%wt. 0.5 +HD 0.5)﹞Diol-2000 was reacted with diphenylmethane-4,4'-diisocyanate (MDI) to prepare a prepolymer with free -NCO%=8.5%, which was then chain extended with a small molecule diol 1,4-butanediol (1,4-BDO) to prepare a polyurethane elastomer sample (transparent). The test performance results showed: Shore A hardness 96, tensile strength 34.8MPa, elongation at break 569.8%, tear strength 158.2KN / m, and impact rebound rate 26%.

[0080] The above description is only for better explaining the embodiments of the present invention, and is not intended to limit the present invention. Any modification or equivalent substitution that does not depart from the spirit and scope of the present invention shall fall within the scope of the present invention.

Claims

1. A method for catalyzing the synthesis of low-polymerization degree polyester polyols using dimethyl oxalate as a raw material, characterized in that: The following steps are involved: Step 1, transesterification reaction stage: under normal pressure, dimethyl oxalate, a small molecule polyol and a catalyst are mixed, and the temperature is raised to a reaction temperature to carry out a transesterification reaction between dimethyl oxalate and the small molecule polyol; Step 2, reduced pressure polyurethane reaction stage: reduce the pressure from normal pressure to high vacuum in stages, and increase the reaction temperature to the set temperature to remove by-products and excess small molecule polyols to achieve the growth of molecular chain segments; after the reaction is completed, cool down to obtain polyester polyols with an average molecular weight of 1000 to 3000.

2. The method for catalyzing the synthesis of low-polymerization degree polyester polyols using dimethyl oxalate as a raw material according to claim 1, characterized in that: In step 1, the small molecule polyol is a straight chain saturated fatty alcohol, the number of its C atoms is 5 to 10, and the hydroxyl functionality is ≥2; or a branched chain saturated fatty alcohol, the number of its C atoms is 4 to 10, and the hydroxyl functionality is ≥2.

3. A method for catalyzing the synthesis of low-polymerization degree polyester polyols using dimethyl oxalate as a raw material according to claim 2, characterized in that: The straight-chain saturated fatty alcohol is one or more of 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, dipropylene glycol, triethylene glycol or tetraethylene glycol; the branched-chain saturated fatty alcohol is one or more of 2-methyl-1,3-propanediol, neopentyl glycol, 1,3-butanediol, 2-ethyl-hexanediol, 3-methyl-1,5-pentanediol, 2,4-diethyl-1,5-pentanediol, 2,2,4-trimethyl-1,3-pentanediol, 2-butyl-2-ethyl-1,3-propanediol, 2-ethyl-1,3-hexanediol, 2-methyl-1,8-octanediol or trimethylolpropane.

4. The method for catalyzing the synthesis of low-polymerization degree polyester polyols using dimethyl oxalate as a raw material according to claim 1, characterized in that: The catalyst in step 1 is one of an organic titanate chelate, an organic tin compound, an organic amine compound, Mg-Al hydrotalcite or a Ca-Zr-Ni based catalyst.

5. The method for catalyzing the synthesis of low-polymerization degree polyester polyols using dimethyl oxalate as a raw material according to claim 4, characterized in that: The organic titanate chelate is one of bis(ethyl acetoacetate) di-n-butoxy titanate chelate, bistriethanolamine diisopropyl titanate chelate, bis(ethyl acetoacetate) diisobutyl titanate chelate, bis(ethyl acetoacetate) diisopropyl titanate chelate, bis(ethyl acetoacetate) diisopropyl titanate chelate, bis(acetylacetonate) ethoxyisopropoxy titanate chelate, bis(acetylacetonate) isobutoxyisopropoxy titanate chelate, and bis(acetylacetonate) diisopropyl titanate chelate.

6. The method for catalyzing the synthesis of low-polymerization degree polyester polyols using dimethyl oxalate as a raw material according to claim 1, characterized in that: The amount of the catalyst used in step 1 is 50ppm to 1000ppm of the mass of the small molecule polyol in the ester exchange reaction stage; the molar ratio of dimethyl oxalate to the small molecule polyol is 1:1 to 2; the temperature of the ester exchange reaction is 130 to 230°C, and the time is 4hr to 12hr.

7. The method for catalyzing the synthesis of low-polymerization degree polyester polyols using dimethyl oxalate as a raw material according to claim 6, characterized in that: The amount of the catalyst used is 100ppm to 300ppm of the mass of the small molecule polyol in the ester exchange reaction stage, the molar ratio of dimethyl oxalate to the small molecule polyol is 1:1 to 1.5, and the ester exchange reaction time is 6hr to 8hr.

8. The method for catalyzing the synthesis of low-polymerization degree polyester polyols using dimethyl oxalate as a raw material according to claim 1, characterized in that: In the step 2, the pressure is reduced from normal pressure to -0.050 MPa to -0.095 MPa in stages, the temperature of the polycondensation reaction is 160° C. to 250° C., and the time is 2 hr to 12 hr.

9. The method for catalyzing the synthesis of low-polymerization degree polyester polyols using dimethyl oxalate as a raw material according to claim 8, characterized in that: The temperature of the polycondensation reaction is 180° C. to 210° C., and the time is 3 hr to 6 hr.

10. Use of the low-polymerization degree polyester polyol prepared by the method according to any one of claims 1 to 9 in the synthesis of polyurethane materials.

Citation Information

Patent Citations

  • Preparation method of high-molecular-weight poly(hexanediol oxalate)

    CN113527644A

  • High molecular weight aliphatic polyoxalate and preparation method thereof

    CN115490838A

  • High-thermal-stability polyethylene glycol oxalate copolyester and preparation method thereof

    CN115785410A

  • Preparation method of poly (dimethyl oxalate) polyol

    CN115819736A