Purification method of terminated polyphenyl ether

Through the esterification reaction and azeotropic evaporation technology of alkyl alcohols and methacrylic acid, the problem of difficult removal of methacrylic acid by-products in the prior art is solved, and a high-purity blocked polyphenylene ether product is realized, which is suitable for high-quality high-quality Frequency high-speed copper clad plate improves dielectric performance.

CN118909243APending Publication Date: 2024-11-08INST OF CHEM ENG GUANGDONG ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411070994.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The prior art is difficult to effectively remove methacrylic acid by-products in thermoset polyphenylene ether resins, resulting in low product purity and easy introduction of sodium ion impurities during washing, affecting the electrical performance and reliability of electronic circuits.

Method used

The esterification reaction is carried out by alkyl alcohol and methacrylic acid in the reaction product solution to form alkyl methacrylate, and the impurity content is reduced by azeotropic evaporation, avoiding the introduction of sodium ions, and achieving high-purity blocked polyphenylene ether product.

Benefits of technology

It significantly reduces the methacrylic impurities content in the end-capped polyphenylene ether, avoids scaling problems, and obtains high-purity products, suitable for high-frequency and high-speed copper clad plates, improving dielectric performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118909243A_ABST
    Figure CN118909243A_ABST
Patent Text Reader

Abstract

The invention discloses a purification method of terminated polyphenyl ether, and relates to the technical field of high-molecular compounds. The purification method comprises the following steps: mixing a reaction product solution of dihydroxy-terminated polyphenyl ether and methacrylic anhydride with alkyl alcohol, carrying out esterification reaction and solid-liquid separation, washing and purifying the obtained solid product with alkyl alcohol, and drying to obtain the end-capped polyphenyl ether finished product. The end-capped polyphenyl ether product obtained by the invention has the characteristic of low impurity content, particularly has lower methacrylic acid content and sodium ion content, can be used for cross-linking and curing with other thermosetting resins to prepare a high-heat-resistance and low-dielectric copper-clad plate material, and can provide more excellent dielectric properties while improving the thermal properties of the material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of polymer compound technology, and in particular to a purification method for end-capped polyphenylene ether. Background Technology

[0002] Thermosetting polyphenylene ether resins are characterized by low viscosity and high reactivity. Through curing with thermosetting resins such as cyanate esters and bismaleimide, the heat resistance and dielectric properties of the material can be significantly improved, making it one of the main resin raw materials for high-frequency, high-speed copper-clad laminates. Besides key indicators such as viscosity and reactivity, high purity is also a fundamental requirement for raw materials in electronic products. The impurity content and ion content of resin raw materials have a crucial impact on the electrical performance and reliability of electronic circuits.

[0003] Typical thermosetting polyphenylene ether resins are end-capped polyphenylene ethers, specifically methacrylate-terminated functionalized polyphenylene ethers, which are formed by modifying the end groups of dihydroxyl-terminated polyphenylene ethers. The traditional preparation method involves reacting dihydroxyl-terminated polyphenylene ethers with methacrylic anhydride in a good solvent under the catalysis of 4-dimethylaminopyridine (DMAP) to form a methacrylate-terminated functionalized polyphenylene ether solution. After precipitation, filtration, washing, and drying, methacrylate-terminated functionalized polyphenylene ether powder is obtained. However, this method suffers from the presence of a large amount of methacrylic acid (MAA) byproduct in the reaction mixture. During precipitation, impurities easily become trapped within the particles, making it difficult to reduce the methacrylic acid content to an ideal level even with repeated washing with large amounts of solvent, resulting in low product purity. Furthermore, during drying, high-boiling-point impurities such as methacrylic acid tend to accumulate and form scale in poorly insulated areas like the dryer, further affecting product purity.

[0004] With the continuous development of integrated circuit technology, the purity requirements for raw materials in applications are becoming increasingly stringent. To improve the purity of capped polyphenylene ether (PPE) products, existing technologies disclose a method for preparing PPE by washing the capping reaction mixture with a concentrated alkaline aqueous solution to remove the capping impurity methacrylic acid. While this method effectively removes the methacrylic acid byproduct through acid-base neutralization, it inevitably introduces sodium ions and generates new wastewater. Furthermore, existing technologies also disclose a method for purifying PPE by contacting the capped PPE solution with a hydrated acidic clay adsorbent to reduce the content of organic acids and organic amines in the product. However, this method introduces the acidic clay adsorbent, which requires repeated regeneration, making the process complex and unable to conveniently and effectively obtain high-purity PPE products. Summary of the Invention

[0005] The present invention aims to at least solve one of the aforementioned technical problems existing in the prior art. Therefore, the object of the present invention is to provide a purification method for capped polyphenylene ethers, which utilizes an alkyl alcohol to react with the capping byproduct to generate an ester, followed by azeotropic distillation, thereby reducing the content of methacrylic acid impurities in the product and improving product purity.

[0006] A second aspect of the present invention is to provide a method for preparing methacrylate-functionalized polyphenylene ether.

[0007] A third aspect of the present invention is to provide an application of the purification method or preparation method described herein.

[0008] To achieve the above objectives, the technical solution adopted by the present invention is as follows:

[0009] A first aspect of the present invention provides a method for purifying capped polyphenylene ether, comprising the following steps:

[0010] The reaction product solution of dihydroxyl-terminated polyphenylene ether and methacrylic anhydride was mixed with an alkyl alcohol and subjected to esterification reaction. After solid-liquid separation, the obtained solid product was washed and purified with an alkyl alcohol and dried to obtain the end-capped polyphenylene ether product.

[0011] End-capped polyphenylene ether (PPE), also known as methacrylate-terminated PPE, typically contains a large amount of the end-capping byproduct methacrylic acid (MAA) in its crude product. This invention utilizes an alkyl alcohol to esterify methacrylic acid in the reaction product solution, generating alkyl methacrylate. After washing to remove a portion of the alkyl methacrylate and alkyl alcohol, they can be further azeotropically evaporated during the drying process. This significantly reduces the methacrylic acid impurity content in the end-capped PPE product, while also preventing the accumulation and scaling of high-boiling-point impurities such as methacrylic acid in the dryer and avoiding the introduction of sodium ion impurities. This allows for a rapid and effective way to obtain high-purity end-capped PPE products.

[0012] Preferably, the reaction product solution contains end-capped polyphenylene ether, methacrylic acid, and end-capped catalyst.

[0013] Preferably, the end-capping catalyst comprises 4-dimethylaminopyridine.

[0014] Preferably, the alkyl alcohol includes one or both of methanol and ethanol.

[0015] Preferably, the mass ratio of the alkyl alcohol to the reaction product solution is (3-15):1.

[0016] More preferably, the mass ratio of the alkyl alcohol to the reaction product solution is (5-7):1.

[0017] Controlling the mass ratio of the reaction product solution to the alkyl alcohol during mixing is beneficial for subsequent esterification reactions.

[0018] Preferably, the esterification reaction is carried out under heating and stirring.

[0019] Preferably, the esterification reaction is carried out at a temperature of 65–90°C.

[0020] More preferably, the temperature of the esterification reaction is 75–90°C.

[0021] In the purification method of the present invention, by further controlling the esterification reaction temperature, it is possible to better ensure the successful esterification reaction of alkyl alcohol and end-capping byproduct methacrylic acid, thereby reducing the impurity content in the subsequent products.

[0022] Preferably, the pressure of the esterification reaction is 0 to 0.15 MPaG.

[0023] More preferably, the pressure of the esterification reaction is 0.05 to 0.15 MPaG.

[0024] Preferably, the esterification reaction takes 0.5 to 5 hours.

[0025] More preferably, the esterification reaction takes 1 to 3 hours.

[0026] Preferably, the drying temperature is 80–120°C.

[0027] More preferably, the drying temperature is 90–110°C.

[0028] The drying temperature is related to the azeotropic distillation of alkyl methacrylates and alkyl alcohols. Further control of the drying temperature is more conducive to the removal of alkyl methacrylates and alkyl alcohols.

[0029] Preferably, the drying is carried out under negative pressure.

[0030] Preferably, the washing includes the following steps: washing and filtering the solid product obtained from the solid-liquid separation with an alkyl alcohol of 1 to 2 times the mass of the solid product, repeating 1 to 2 times.

[0031] Preferably, the solid product obtained from the solid-liquid separation contains 45-55% by mass of capped polyphenylene ether solid.

[0032] In this invention, regardless of whether centrifugation or filtration is used for solid-liquid separation, the final solid product is always a wet solid containing 45-55 wt% end-capped polyphenylene ether solids, with a high moisture content. Therefore, repeated washing and purification with alkyl alcohols alone is not very efficient. By employing the method of this invention to perform an esterification reaction before washing and purification, the impurity content of the final product can be effectively reduced.

[0033] Preferably, after the reaction product solution is mixed with an alkyl alcohol, a solid precipitates out. After initial solid-liquid separation, the resulting slurry is subjected to an esterification reaction.

[0034] Preferably, the slurry comprises the following components in weight percentage: 25-40 wt% capped polyphenylene ether, 0.2-2 wt% methacrylic acid, and 0.04-0.4 wt% capping catalyst.

[0035] More preferably, the slurry comprises the following components in weight percentage: 25-35 wt% capped polyphenylene ether, 0.4-2 wt% methacrylic acid, and 0.04-0.1 wt% capped catalyst.

[0036] The remaining amount of the slurry includes alkyl alcohols, unreacted raw materials, and organic solvents; the organic solvent may be toluene.

[0037] Preferably, the reaction product solution is concentrated by evaporation before being mixed with the alkyl alcohol.

[0038] Preferably, the content of methacrylic acid in the end-capped polyphenylene ether product is ≤500ppm.

[0039] More preferably, the content of methacrylic acid in the end-capped polyphenylene ether product is 150-400 ppm.

[0040] Preferably, the content of alkyl methacrylate in the end-capped polyphenylene ether product is ≤100ppm.

[0041] More preferably, the content of alkyl methacrylate in the end-capped polyphenylene ether product is 20-90 ppm.

[0042] Preferably, the content of the end-capping catalyst in the end-capped polyphenylene ether product is ≤500ppm.

[0043] More preferably, the content of the end-capping catalyst in the end-capped polyphenylene ether product is 150-300 ppm.

[0044] Preferably, the sodium ion content in the end-capped polyphenylene ether product is ≤10ppm.

[0045] More preferably, the sodium ion content in the end-capped polyphenylene ether product is 5-10 ppm.

[0046] Preferably, the intrinsic viscosity of the end-capped polyphenylene ether product is 0.05 dl / g to 0.25 dl / g.

[0047] Preferably, the double-hydroxyl-terminated polyphenylene ether has the structure shown in formula (Ⅰ):

[0048]

[0049] In formula (Ⅰ), R1, R2, R3, R4, R5, and R6 independently represent hydrogen atoms, alkyl groups, phenyl groups, alkoxy groups, halogens, or haloalkyl groups, respectively; m is an integer from 0 to 60; and n is an integer from 0 to 60.

[0050] Preferably, the hydroxyl content of the double-hydroxyl-terminated polyphenylene ether is 0.25 mmol / g to 2.5 mmol / g.

[0051] More preferably, the hydroxyl content of the dihydroxyl-terminated polyphenylene ether is 0.3 mmol / g to 1.5 mmol / g.

[0052] Preferably, the number-average molecular weight of the dihydroxyl-terminated polyphenylene ether is 1500 to 6000.

[0053] Preferably, after the esterification reaction, the conversion rate of methacrylic acid is ≥70%.

[0054] More preferably, after the esterification reaction, the conversion rate of methacrylic acid is 70-95%.

[0055] A second aspect of the present invention provides a method for preparing end-capped polyphenylene ether, comprising the following steps:

[0056] A solution of hydroxyl-terminated polyphenylene ether was mixed with methacrylic anhydride and a capping catalyst to carry out a capping reaction, thereby obtaining a reaction product solution.

[0057] The reaction product solution was purified to obtain the capped polyphenylene ether product;

[0058] The purification method is the purification method described in the first aspect of this invention.

[0059] Preferably, the hydroxyl-terminated polyphenylene ether solution comprises hydroxyl-terminated polyphenylene ether and its good solvent.

[0060] More preferably, the hydroxyl-terminated polyphenylene ether solution is a toluene solution of hydroxyl-terminated polyphenylene ether.

[0061] Preferably, the molar ratio of the methacrylic anhydride to the hydroxyl groups in the dihydroxyl-terminated polyphenylene ether is (1-3):1.

[0062] More preferably, the molar ratio of the methacrylic anhydride to the hydroxyl groups in the dihydroxyl-terminated polyphenylene ether is (1.2-2):1.

[0063] Preferably, the molar ratio of the end-capping catalyst to the hydroxyl groups in the bihydroxyl-terminated polyphenylene ether is (0.06-0.20):1.

[0064] More preferably, the molar ratio of the end-capping catalyst to the hydroxyl groups in the bihydroxyl-terminated polyphenylene ether is (0.08-0.15):1.

[0065] Preferably, the reaction temperature of the end-capping reaction is 80–120°C.

[0066] More preferably, the reaction temperature of the end-capping reaction is 90–110°C.

[0067] Preferably, the end-capping reaction takes 2 to 6 hours.

[0068] More preferably, the end-capping reaction takes 3 to 5 hours.

[0069] The third aspect of the present invention provides an application of the purification method of the end-capped polyphenylene ether described in the first aspect of the present invention or the preparation method of the end-capped polyphenylene ether described in the second aspect of the present invention in the preparation of copper-clad laminates.

[0070] In some embodiments of the present invention, the copper-clad laminate is a high-frequency, high-speed copper-clad laminate.

[0071] Compared with the prior art, the beneficial effects of the present invention are:

[0072] (1) The present invention provides a purification method for capped polyphenylene ether. The purification method uses alkyl alcohol as a precipitant to cause the high-boiling-point capping byproduct methacrylic acid in the crude capped polyphenylene ether to undergo an esterification reaction with the alkyl alcohol at a certain temperature to generate alkyl methacrylate. During the drying process, the generated alkyl methacrylate is azeotropically distilled off with the alkyl alcohol, thereby greatly reducing the content of methacrylic acid impurities in the finished capped polyphenylene ether and also avoiding the accumulation and scaling of high-boiling-point impurities such as methacrylic acid in the dryer.

[0073] (2) The end-capped polyphenylene ether obtained by the present invention has a low impurity content, especially a low methacrylic acid content and sodium ion content. The methacrylic acid content is ≤500ppm, the alkyl methacrylate content is ≤100ppm, the end-capping catalyst content is ≤500ppm, and the sodium ion content is ≤10ppm. It is particularly suitable for preparing high-frequency and high-speed copper-clad laminates and can give the products better dielectric properties. Attached Figure Description

[0074] Figure 1 The image shows the H-ray nuclear magnetic resonance spectrum of the end-capped polyphenylene ether product obtained in Example 1.

[0075] Figure 2 This is an enlarged view of the nuclear magnetic resonance H-ray spectrum of the capped polyphenylene ether product obtained in Example 1. Detailed Implementation

[0076] The present invention will be further described in detail below through specific embodiments. Unless otherwise specified, the raw materials, reagents, or apparatus used in the embodiments and comparative examples are all available from conventional commercial sources or can be obtained by existing technical methods. Unless otherwise specified, the test or experimental methods are conventional methods in the art.

[0077] The preparation method of the dihydroxy polyphenylene ether solution A used in the following Examples 1-2 and Comparative Examples 1-3 of the present invention includes the following steps:

[0078] 1) Add 250.0 kg of 2,6-dimethylphenol, 52.5 kg of tetramethylbisphenol A, and 1000.0 kg of toluene to the reactor. Stir until all monomers are dissolved. Then add 3.8 kg of di-n-butylamine, 11.3 kg of N,N-dimethylbutylamine, and 2.0 kg of copper bromide. Mix thoroughly and then purge with oxygen (15.0 Nm³). 3 / h), react at 40℃ for 200 min;

[0079] 2) After the reaction is complete, add 37.5 kg of 5% sodium ethylenediaminetetraacetate aqueous solution, stir at 70°C for 60 min, and then centrifuge to remove the aqueous phase to obtain dihydroxy polyphenylene ether solution A.

[0080] The preparation method of the dihydroxy polyphenylene ether solution B used in the following Examples 3-4 of the present invention includes the following steps:

[0081] 1) Add 100.0 kg 2,6-dimethylphenol, 5.0 kg tetramethylbisphenol A, and 400.0 kg toluene to the reactor. Stir until all monomers are dissolved. Then add 1.5 kg di-n-butylamine, 4.5 kg N,N-dimethylbutylamine, and 0.8 kg copper bromide. Mix thoroughly and then introduce oxygen (6.0 Nm³). 3 / h), react at 40℃ for 240min;

[0082] 2) After the reaction is complete, add 15 kg of 5% sodium ethylenediaminetetraacetate aqueous solution, stir at 70°C for 60 min, and then centrifuge to remove the aqueous phase to obtain dihydroxy polyphenylene ether solution B.

[0083] 50g each of dihydroxyphenylene ether solution A and dihydroxyphenylene ether solution B were placed in flasks, concentrated by rotary evaporation, and then dried under vacuum at 100℃ in a drying oven to obtain dihydroxyphenylene ether A and dihydroxyphenylene ether B, respectively. The solid contents of dihydroxyphenylene ether solution A and dihydroxyphenylene ether solution B were calculated to be 23.5% and 21.0%, respectively, based on the weight changes of the samples before and after drying.

[0084] The number-average molecular weight of the dried solid samples was determined using gel permeation chromatography, and the hydroxyl content was determined using proton nuclear magnetic resonance spectroscopy. The test results are shown in Table 1.

[0085] Table 1 Performance test results of dihydroxyphenylene ether A and dihydroxyphenylene ether B samples

[0086] sample Number average molecular weight Hydroxyl content (mmol / g) Dihydroxy polyphenylene ether A 1625 1.20 Dihydroxy polyphenylene ether B 5921 0.33

[0087] The preparation method of the reaction product solution in Example 1 of the present invention is as follows:

[0088] 13.9 kg of methacrylic anhydride and 0.7 kg of 4-dimethylaminopyridine (DMAP) were added to 212.8 kg of dihydroxy-terminated polyphenylene ether solution A, and the reaction was carried out at 100 °C for 4 h to obtain the reaction product solution.

[0089] The preparation method of the reaction product solution in Example 2 of the present invention is as follows:

[0090] 13.9 kg of methacrylic anhydride and 0.7 kg of 4-dimethylaminopyridine were added to 212.8 kg of dihydroxyl-terminated polyphenylene ether solution A, and the reaction was carried out at 100 °C for 4 h to obtain the reaction product solution.

[0091] The preparation method of the reaction product solution in Example 3 of the present invention is as follows:

[0092] Add 3.9 kg of methacrylic anhydride and 0.3 kg of 4-dimethylaminopyridine to 238.1 kg of dihydroxyl-terminated polyphenylene ether solution A, and react at 100 °C for 4 h to obtain the reaction product solution.

[0093] The preparation method of the reaction product solution in Example 4 of the present invention is as follows:

[0094] Add 3.9 kg of methacrylic anhydride and 0.3 kg of 4-dimethylaminopyridine to 238.1 kg of dihydroxyl-terminated polyphenylene ether solution A, and react at 100 °C for 4 h to obtain the reaction product solution.

[0095] Example 1

[0096] This embodiment provides a purification method for capped polyphenylene ether, including the following steps:

[0097] 1) The reaction product solution was heated and evaporated to concentrate, and 100.0 kg of toluene was distilled off; the concentrated reaction product solution was added to 700.7 kg of methanol and stirred to precipitate the end-capped polyphenylene ether, thus obtaining a mixed solution.

[0098] 2) Add all the mixed liquid obtained in step 1) into the filter washing dryer and filter out 647.2 kg of liquid to obtain filtrate A and slurry (solid content of 30 wt%). Stir the obtained slurry at 0.1 MPaG and 80℃ for 2 h to allow the methacrylic acid (MAA) in the slurry to undergo an esterification reaction with methanol to generate methyl methacrylate (AMA). After the reaction is completed, cool the material to below 55℃.

[0099] 3) The cooled slurry was further filtered to obtain 67.2 kg of liquid and filtrate B and the end-capped polyphenylene ether solid product. 170.0 kg of methanol was added to the solid product, and the mixture was pulped, washed, filtered, and repeated once (i.e., washed twice). The obtained solid product was then vacuum dried at 100°C for 12 h to obtain end-capped polyphenylene ether powder.

[0100] Example 2

[0101] This embodiment provides a purification method for methacrylate-functionalized polyphenylene ether, including the following steps:

[0102] 1) The reaction product solution was heated and evaporated to concentrate, and 100.0 kg of toluene was distilled off; the concentrated reaction product solution was added to 778.6 kg of methanol and stirred to precipitate the end-capped polyphenylene ether, thus obtaining a mixed solution.

[0103] 2) Add all the mixed liquid obtained in step 1) into the filter washing dryer and filter out 751.0 kg of liquid (filtrate A) to obtain slurry (solid content of 35 wt%). Stir the obtained slurry at 0.05 MPaG and 75°C for 3 h to allow the methacrylic acid in the slurry to undergo an esterification reaction with methanol to generate methyl methacrylate. After the reaction is completed, cool the material to below 55°C.

[0104] 3) The cooled slurry was further filtered to obtain 40.0 kg of liquid (filtrate B) and a solid product of capped polyphenylene ether was obtained. 170.0 kg of methanol was added to the solid product, and the mixture was pulped, washed, filtered, and repeated once (i.e., washed twice). The obtained solid product was then vacuum dried at 90°C for 15 h to obtain capped polyphenylene ether powder.

[0105] Example 3

[0106] This embodiment provides a purification method for capped polyphenylene ether, including the following steps:

[0107] 1) The reaction product solution was heated and evaporated to concentrate, and 100.0 kg of toluene was distilled off; the concentrated reaction product solution was added to 722.4 kg of methanol and stirred to precipitate the end-capped polyphenylene ether, thus obtaining a mixed solution.

[0108] 2) Add all the mixed liquid obtained in step 1) into the filter washing dryer and filter out 660.2 kg of liquid (filtrate A) to obtain slurry (solid content of 25 wt%). Stir the obtained slurry at 0.13 MPaG and 85℃ for 2 h to allow the methacrylic acid in the slurry to undergo an esterification reaction with methanol to generate methyl methacrylate. After the reaction is completed, cool the material to below 55℃.

[0109] 3) The cooled slurry was further filtered to obtain 96.0 kg of liquid (filtrate B) and a solid product of capped polyphenylene ether was obtained. 170.0 kg of methanol was added to the solid product, and the mixture was pulped, washed, filtered, and repeated once (i.e., washed twice). The obtained solid product was vacuum dried at 110°C for 10 h to obtain capped polyphenylene ether powder.

[0110] Example 4

[0111] This embodiment provides a purification method for capped polyphenylene ether, including the following steps:

[0112] 1) The reaction product solution was heated and evaporated to concentrate, and 100.0 kg of toluene was distilled off; the concentrated reaction product solution was added to 828.1 kg of ethanol and stirred to precipitate the end-capped polyphenylene ether, thus obtaining a mixed solution.

[0113] 2) Add all the mixed liquid obtained in step 1) into the filter washing and drying machine, filter out 800.0 kg of liquid (filtrate A) to obtain slurry (solid content is 30 wt%), stir the obtained slurry at 0.05 MPaG and 88℃ for 2 h to allow the methacrylic acid in the slurry to undergo esterification reaction with ethanol to generate ethyl methacrylate. After the reaction is completed, cool the material to below 65℃.

[0114] 3) The cooled slurry was further filtered to obtain 62.0 kg of liquid (filtrate B) and a solid product of end-capped polyphenylene ether was obtained. 170.0 kg of methanol was added to the solid product, and the mixture was pulped, washed, filtered, and repeated once (i.e., washed twice). The obtained solid product was vacuum dried at 110°C for 10 h to obtain end-capped polyphenylene ether powder.

[0115] Examples 5-9

[0116] This embodiment provides a purification method for end-capped polyphenylene ether, which differs from Example 1 only in that the esterification reaction temperature and pressure are 65℃ and 0.02MPa (Example 5); 70℃ and 0.05MPa (Example 6); 75℃ and 0.07MPa (Example 7); 85℃ and 0.15MPa (Example 8); and 90℃ and 0.20MPa (Example 9).

[0117] Comparative Example 1

[0118] This comparative example provides a method for preparing and purifying end-capped polyphenylene ether, including the following steps:

[0119] 1) Add 13.9 kg of methacrylic anhydride and 0.7 kg of 4-dimethylaminopyridine to 212.8 kg of dihydroxyl-terminated polyphenylene ether solution A, and perform end-capping reaction at 100 °C for 4 h; heat and evaporate the product solution obtained from the reaction to concentrate it, and distill off 100.0 kg of toluene; add the concentrated solution to 700.7 kg of methanol and stir to precipitate the end-capped polyphenylene ether, and obtain a mixed solution;

[0120] 2) Add all the mixture from step 1) into a filter washing dryer and filter out 715.3 kg of liquid to obtain a solid product of capped polyphenylene ether; add 170.0 kg of methanol to the solid product, slurry and wash, filter, repeat once (i.e. wash twice), and vacuum dry the obtained solid product at 100℃ for 12 h to obtain capped polyphenylene ether powder.

[0121] Comparative Example 2

[0122] This comparative example provides a method for preparing and purifying end-capped polyphenylene ether, including the following steps:

[0123] 1) Add 13.9 kg of methacrylic anhydride and 0.7 kg of 4-dimethylaminopyridine to 212.8 kg of dihydroxyl-terminated polyphenylene ether solution A, and perform end-capping reaction at 100 °C for 4 h; heat and evaporate the product solution obtained from the reaction to concentrate it, and distill off 100.0 kg of toluene; add the concentrated solution to 700.7 kg of methanol and stir to precipitate the end-capped polyphenylene ether, and obtain a mixed solution;

[0124] 2) Add all the mixture from step 1) into a filter washing dryer, filter out 714.8 kg of liquid, and obtain a solid product of capped polyphenylene ether. Add 170.0 kg of methanol to the solid product, heat to 80°C under 0.1 MPaG pressure and stir for 2 hours (equivalent to esterification reaction during the first washing process), and then cool the material to below 55°C.

[0125] 3) The cooled slurry was further filtered to obtain a solid product of end-capped polyphenylene ether; 170.0 kg of methanol was added to the solid product, the slurry was pulverized and washed, filtered, and the obtained solid product was vacuum dried at 100℃ for 12 h to obtain end-capped polyphenylene ether powder.

[0126] Comparative Example 3

[0127] This comparative example provides a method for preparing and purifying end-capped polyphenylene ether, including the following steps:

[0128] 1) Add 13.9 kg of methacrylic anhydride and 0.7 kg of 4-dimethylaminopyridine to 212.8 kg of dihydroxyl-terminated polyphenylene ether solution A, and perform end-capping reaction at 100 °C for 4 h; add 24 kg of 30% sodium hydroxide solution to the product solution obtained from the reaction, stir for 0.5 h, and allow to stand for phase separation to remove the aqueous phase; add 24 kg of deionized water, stir and wash for 0.5 h, allow to stand for phase separation to remove the aqueous phase, and repeat the water washing once; heat and evaporate the washed solution to concentrate, and distill off 100.0 kg of toluene; add the concentrated solution to 700.7 kg of methanol and stir to mix, so that the end-capped polyphenylene ether precipitates, and obtain a mixed solution;

[0129] 2) Add all the mixture from step 1) into a filter washing dryer and filter out 715.3 kg of liquid to obtain a solid product of capped polyphenylene ether; add 170.0 kg of methanol to the solid product, slurry and wash, filter, repeat once (i.e. wash twice), and vacuum dry the obtained solid product at 100℃ for 12 h to obtain capped polyphenylene ether powder.

[0130] Result detection

[0131] The contents of methacrylic acid and 4-dimethylaminopyridine in filtrate A were determined by gas chromatography, and the contents of methacrylic acid and 4-dimethylaminopyridine in the slurry were calculated.

[0132] Take 1g of the slurry obtained after the esterification reaction in step 2) of Examples 1 to 4 respectively, dissolve it in 50mL of toluene, test the content of methacrylic acid and alkyl methacrylate by gas chromatography, convert the test value into the molar amount of the two, and calculate the conversion rate of methacrylic acid.

[0133] The intrinsic viscosity of the end-capped polyphenylene ether powder was tested at 30°C using chloroform as a solvent and an Ubbelohde viscometer.

[0134] Detailed parameters and test results for Examples 1-4 are shown in Table 3:

[0135] Table 3 Detailed parameters and test results for Examples 1-4

[0136]

[0137]

[0138] The impurity content of the end-capped polyphenylene ether products obtained from Examples 1-9 and Comparative Examples 1-3 was tested using the following methods:

[0139] 1 g of the obtained end-capped polyphenylene ether powder was dissolved in 50 mL of toluene, and the contents of methacrylic acid, methyl methacrylate, and 4-dimethylaminopyridine in the product were tested by gas chromatography. The obtained end-capped polyphenylene ether powder was subjected to microwave digestion pretreatment, and then the sodium ion content of the product was tested by ICP-MS.

[0140] The results are compared in Tables 4 and 5 below:

[0141] Table 4. Test results of impurity content in end-capped polyphenylene ether powders from Examples 1 and 5-9.

[0142] project Example 1 Example 5 Example 6 Example 7 Example 8 Example 9 MAA content / ppm 282 960 532 388 273 250 AMA content / ppm 83 67 77 83 86 87 DMAP content / ppm 273 281 230 283 295 287 Sodium ion content / ppm 8 9 6 8 7 7

[0143] Table 5. Test results of impurity content in end-capped polyphenylene ether powders from Examples 1-4 and Comparative Examples 1-3.

[0144] project Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 Comparative Example 3 MAA content / ppm 282 353 238 150 3684 1845 325 AMA content / ppm 83 87 24 21 0 64 0 DMAP content / ppm 273 246 162 151 295 287 221 Sodium ion content / ppm 8 6 7 7 8 8 348

[0145] As can be seen from Table 4, when the temperature of the esterification reaction increases from 65℃ to 90℃, the MAA content in the resulting capped polyphenylene ether product decreases. When the temperature is higher than 75℃, the MAA content can reach below 500ppm, while the AMA, DMAP and sodium ion contents do not show obvious changing trends.

[0146] As shown in Table 5, Comparative Example 1, a traditional purification method for capped polyphenylene ether, involves directly filtering, washing, and drying the capped polyphenylene ether slurry mixed with methanol. The resulting product has a MAA content as high as 3684 ppm, significantly higher than the MAA content of the product obtained by the method of this invention. Although AMA impurities are present in the product after using the method of this invention, their content is extremely low, and the MAA and total AMA content are still significantly reduced in comparison.

[0147] In Comparative Example 2, the mixture of capped polyphenylene ether (PPE) and methanol was directly filtered to obtain a wet PPE sample. After adding methanol, a heating esterification reaction was performed during the first washing process. Although the MAA content of the resulting product was lower than that of Comparative Example 1, it was still higher than that of the product prepared by the method of this invention. This indicates that in the purification method of this invention, esterification of the slurry is more conducive to the conversion of MAA to AMA compared to reacting the solid obtained by direct filtration with methanol. Furthermore, esterification during the washing process results in a lower DMAP catalyst concentration, which is detrimental to the conversion of MAA.

[0148] Comparative Example 3 used sodium hydroxide solution to wash away MAA after the reaction, and then carried out further purification. The MAA content of the obtained product was significantly lower than that of Comparative Examples 1 and 2. However, sodium ion impurities were inevitably introduced, with a sodium ion content as high as 348 ppm, which could not meet the requirements for application in high-frequency and high-speed copper-clad laminates.

[0149] Figure 1 The image shown is the H-NMR spectrum of the capped polyphenylene ether prepared in Example 1 of this invention. Figure 2 Enlarge the image. Combined with... Figure 1 and Figure 2 It can be seen that peak 1 at 6.98 ppm is the proton peak on the benzene ring of the tetramethylbisphenol A unit, peak 2 at 6.48 ppm is the proton peak on the benzene ring of the repeating unit of polyphenylene ether, and peaks 3 at 6.37 ppm and 4 at 5.74 ppm are the proton peaks of the =CH2 group on the methpropylene group at the end of the molecular chain, respectively. In addition, the proton peak at 3.76 ppm is the proton peak of the methyl methacrylate -OCH3 group, indicating that the obtained end-capped polyphenylene ether contains methyl methacrylate.

[0150] In summary, the method of this invention yields a polyphenylene ether product with a methacrylic acid content below 500 ppm, an alkyl methacrylate content below 100 ppm, a 4-dimethylaminopyridine content below 500 ppm, and a sodium ion content below 10 ppm. Furthermore, compared to conventional methods, the purification method of this invention significantly improves the scaling problem in areas of the filter, washer, and dryer where insulation is poor.

[0151] The end-capped polyphenylene ether product obtained by this invention has the characteristics of low impurity content, especially low methacrylic acid content and sodium ion content. It can be used to cross-link and cure with other thermosetting resins to prepare high heat-resistant and low dielectric copper-clad laminate materials, which can improve the thermal properties of the material and provide better dielectric properties.

[0152] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be considered as equivalent replacement methods and are included in the scope of protection of the present invention.

Claims

1. A method for purifying blocked polyphenylene ether, It is characterized in that The steps include: The reaction product solution of double-terminated hydroxyl polyphenyl ether and methacrylic anhydride is mixed with alkyl alcohol, and esterification reaction is carried out. The solid-liquid separation is performed, and the obtained solid product is then washed and purified with alkyl alcohol and dried to obtain the end-capped polyphenyl ether finished product.

2. The purification method according to claim 1, It is characterized in that The reaction product solution comprises blocked polyphenylene ether, methacrylic acid, and blocked catalyst; And / or, the alkyl alcohol includes one or both of methanol and ethanol.

3. The purification method according to claim 1, It is characterized in that The mass ratio of the alkyl alcohol to the reaction product solution is (3-15):

1.

4. The purification method according to claim 1, It is characterized in that The esterification reaction is carried out under heating and stirring; And / or, the temperature of the esterification reaction is 75-90°C; And / or, the pressure of the esterification reaction is 0 to 0.15 MPaG; And / or, the esterification reaction time is 0.5 to 5 hours; And / or, the drying temperature is 80-120°C.

5. The purification method according to claim 1 or 2, It is characterized in that The reaction product solution is mixed with an alkyl alcohol to precipitate a solid, and after a primary solid-liquid separation, the obtained slurry is subjected to an esterification reaction; And / or, the slurry comprises the following components in percentage by weight: 25-40 wt % of blocked polyphenylene ether, 0.2-2 wt % of methacrylic acid, and 0.04-0.4 wt % of blocked catalyst.

6. The purification method according to claim 1 or 2, It is characterized in that The content of methacrylic acid in the finished blocked polyphenylene ether product is ≤500ppm; And / or, the content of alkyl methacrylate in the finished blocked polyphenylene ether is ≤100ppm; And / or, the content of the blocking catalyst in the blocked polyphenylene ether product is ≤500ppm; And / or, the content of sodium ions in the finished blocked polyphenylene ether product is ≤10ppm.

7. The purification method according to claim 1 or 2, It is characterized in that The intrinsic viscosity of the finished end-capped polyphenylene ether is 0.05 dl / g to 0.25 dl / g.

8. The purification method according to claim 1, It is characterized in that The structure of the double-terminated hydroxyl polyphenylene ether is shown in formula (I): In formula (I), R 1 , R 2 , R 3 , R 4 , R 5 , R 6 Each independently represents a hydrogen atom, an alkyl group, a phenyl group, an alkoxy group, a halogen group or a halogenated alkyl group; m is an integer of 0 to 60; and n is an integer of 0 to 60.

9. A method for preparing a capped polyphenylene ether, It is characterized in that The steps include: The dihydroxy-terminated polyphenylene ether solution is mixed with methacrylic anhydride and a capping catalyst to perform a capping reaction to obtain a reaction product solution; Purifying the reaction product solution to obtain the blocked polyphenylene ether finished product; The purification method is the purification method according to any one of claims 1 to 8.