High-strength and high-toughness biomass material and preparation method thereof
By mixing biomass with water and ionic liquid, and heating, dehydration and solidification treatment, a high-toughness biomass gel material is prepared, which solves the problem of low toughness of the primary biomass material and realizes the preparation of high-strength and high-toughness materials. And the process is environmentally friendly and low cost.
Patent Information
- Application Number
- CN202310510628.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-08
- Publication Date
- 2024-11-08
AI Technical Summary
The existing technology is difficult to prepare high-strength and high-tough biomass materials, especially proto-biomass raw materials. The existence of lignin, hemicellulose and other components leads to low toughness of the material, and plasticizers are often required to improve toughness. Limited effect.
By mixing biomass with water and adding ionic liquid, heating, dehydrating and applying pressure, putting it in a solidification bath to solidify, and finally washing and drying, a high toughness biomass gel material can be prepared. at 15% elongation.
It realizes high strength and toughness of biomass materials without the need for plasticizers, simple process, low cost and environmentally friendly, and is suitable for high-value utilization of biomass.
Smart Images

Figure CN118909275A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of materials and natural polymers, and in particular, relates to a method for preparing a biomass material. Background Art
[0002] Biomass resources come from nature, have huge reserves, and are completely biodegradable. Their effective use is of great significance for protecting the environment and reducing carbon emissions. However, common natural biomass materials are difficult to shape, and even if they are shaped, the resulting materials usually have poor toughness. For example: regenerated cellulose film, trade name cellophane, has a tensile elongation at break of less than 10% without adding plasticizer. When 10-20% glycerol is added as a plasticizer, its tensile elongation at break will increase, but it will still not exceed 20%.
[0003] When natural biomass is used as raw material, due to the presence of multiple components such as lignin, hemicellulose, and inorganic substances, the resulting all-biomass material is usually difficult to shape and has lower toughness. Through delignification and pressure compression, some people have prepared high-strength lignocellulose materials in the prior art, but the toughness is less than 2.5%. Some people have also prepared high-strength cellulose nanocomposites using cellulose nanofibers and mica sheets, but the toughness is less than 1.5%. For example, some people have proposed to prepare high-strength and tough cellulose hydrogels and films by chemical crosslinking first and then physical crosslinking, but this method has only been successfully applied to the NaOH / urea system and cannot be applied to native biomass raw materials. Therefore, developing new methods to prepare high-strength and high-toughness biomass materials has become a technical problem that needs to be solved urgently. Summary of the invention
[0004] In order to improve the above technical problems, the present invention provides a biomass material and a preparation method thereof, wherein the preparation method of the biomass material comprises the following steps:
[0005] Step 1: mixing the biomass with or without light treatment with water to obtain a biomass dispersion;
[0006] Step 2: Add ionic liquid to the biomass dispersion and stir to mix evenly;
[0007] Step 3: heating and dehydrating the biomass / water / ionic liquid mixture until no obvious water evaporates from the mixture, applying pressure;
[0008] Step 4: placing the material obtained in step 3 in a coagulation bath for coagulation to obtain a biomass gel;
[0009] Step 5: Gel the biomass, wash and dry.
[0010] In one embodiment of the present invention, the biomass is selected from the group consisting of films, fibers, and boards.
[0011] Preferably, the biomass is selected from plant straw, grass plants, various wood chips, and agricultural and forestry wastes.
[0012] For example, one or more of cellulose, chitosan, starch, chitin, wheat straw, corn straw, cotton straw, Chinese medicine residues, foxtail grass, pennisetum, barnyard grass, reed, corn cob, bagasse, fruit shells, plant stems and leaves, waste wood chips, wood powder, sawdust, and bamboo powder.
[0013] Preferably, the cellulose is selected from one or more of microcrystalline cellulose, cotton pulp, refined cotton, defatted cotton, wood pulp, cotton linter, bamboo pulp, straw pulp and bacterial cellulose.
[0014] In one embodiment of the present invention, the light treatment is at least one of an alkaline solution treatment, a peracetic acid aqueous solution treatment, a p-toluenesulfonic acid aqueous solution treatment, and an acetic acid / NaClO2 aqueous solution treatment method.
[0015] In one embodiment of the present invention, in step 1, the biomass and water are mixed by stirring or beating to prepare a biomass water dispersion.
[0016] Preferably, the ratio of biomass to water is 1% to 30%, preferably 3% to 20%.
[0017] In one embodiment of the present invention, the ionic liquid is a molten salt formed by a substituted or unsubstituted imidazole or pyridinium cation and an anion having a melting point below 100°C;
[0018] Preferably, the substituent on the imidazole or pyridinium cation is C 1-6 Alkyl, C 1-6 The anion is at least one of an alkyl acid ion, a halide ion, and an organic phosphate ion.
[0019] For example, the ionic liquid is selected from at least one of allyl-3-methylimidazolium chloride (AmimCl), 1-butyl-3-methylimidazolium acetate (BmimAc) ionic liquid and 1-ethyl-3-methylimidazolium acetate (EmimAc).
[0020] In one embodiment of the present invention, the mass ratio of the ionic liquid to the biomass is 13:7 to 17:3, preferably 7:3 to 8:2, for example, 3:1, 3.1:1, 3.2:1, 3.3:1, 3.4:1, 3.5:1, 3.6:1, 3.7:1, 3.8:1, 3.9:1, 4.0:1 and any range or ratio between any of the above points.
[0021] In one embodiment of the present invention, the temperature of heating and dehydration in step 3 is 60-110°C, preferably 80-110°C, for example, 80°C, 85°C, 90°C, 95°C, 100°C, 105°C, 110°C and any range or ratio between any of the above points.
[0022] Preferably, step 3 comprises pressurizing at 0.5 MPa to 5 MPa for 3 min at 80 to 110° C., for example, pressurizing at 0.5 MPa for 3 min at 80° C.
[0023] In one embodiment of the present invention, the coagulation bath is any one of water, alcohol, a mixture of water and an ionic liquid, and a mixture of alcohol and an ionic liquid.
[0024] For example, the alcohol is selected from at least one of ethanol, methanol, isopropanol, n-propanol and n-butanol.
[0025] Preferably, when the coagulation bath is a mixture of water and an ionic liquid, the mass ratio of water to the ionic liquid in the mixture is 1:(0.1-4).
[0026] For example, 1:0.1, 1:0.15, 1:0.2, 1:0.25, 1:0.3, 1:0.35, 1:0.4, 1:0.45, 1:0.5, 1:0.55, 1:0.6, 1:0.65, 1:0.67, 1:1, 1:1.5, 1:2, 1:2.5, 1:3, 1:3.5, 1:4 or the range between any two of the above values.
[0027] Preferably, when the coagulation bath is a mixture of alcohol and ionic liquid, the mass ratio of the alcohol to the ionic liquid in the mixture is 1:(0.1-4).
[0028] For example, 1:0.1, 1:0.15, 1:0.2, 1:0.25, 1:0.3, 1:0.35, 1:0.4, 1:0.45, 1:0.5, 1:0.55, 1:0.6, 1:0.65, 1:0.67, 1:1, 1:1.5, 1:2, 1:2.5, 1:3, 1:3.5, 1:4 or the range between any two of the above values.
[0029] In one embodiment of the present invention, the temperature of the coagulation bath can be 0°C to 50°C, preferably 0°C to 40°C, for example 0°C, 5°C, 10°C, 15°C, 20°C, 25°C, 30°C, 35°C, 40°C or a range between any two of the above values.
[0030] According to another aspect of the present invention, a biomass material is provided, which is obtained by the above-mentioned method for preparing the biomass material.
[0031] Preferably, the biomass material has high toughness, and without adding a plasticizer, the elongation at break exceeds 15%.
[0032] Beneficial effects of the present invention:
[0033] The present invention provides a new biomass processing and molding method for raw biomass raw materials. In the preparation process, high-strength and high-toughness biomass materials can be obtained without adding plasticizers. Without adding plasticizers, the elongation at break exceeds 15%, which is higher than commercial cellophane (containing 10-15% plasticizer). In addition, the preparation method is simple in process, low in cost, environmentally friendly, and pollution-free, which is of great significance for realizing the high-value utilization of biomass. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 This is a scanning electron microscope photograph of the cellulose hydrogel prepared in Comparative Example 1.
[0035] Figure 2 This is the tensile curve of the cellulose film prepared in Comparative Example 1.
[0036] Figure 3 This is a scanning electron microscope photograph of the cross section of the cellulose film prepared in Comparative Example 1 before and after stretching.
[0037] Figure 4 This is an optical photograph of the cellulose hydrogel prepared in Example 1.
[0038] Figure 5 This is a scanning electron microscope photograph of the cellulose hydrogel prepared in Example 1.
[0039] Figure 6 Schematic diagram of the stretching curve of the cellulose film prepared in Example 1.
[0040] Figure 7 The following are scanning electron microscope photographs of the cross section of the cellulose film prepared in Example 1 before and after stretching.
[0041] Figure 8 This is an optical photograph of the straw film prepared in Example 2.
[0042] Fig. 9 This is the infrared spectrum of the straw film prepared in Example 2.
[0043] Fig.10 This is a comparison chart of the tensile toughness of the straw film in Example 2, commercial cellophane, and a straw film prepared by a conventional dissolution regeneration method (see the comparative example for the preparation method). DETAILED DESCRIPTION
[0044] The technical scheme of the present invention will be further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only exemplary descriptions and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are included in the scope that the present invention is intended to protect.
[0045] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.
[0046] Comparative Example 1
[0047] Wood pulp was selected as the raw material. 95 g of 1-ethyl-3-methylimidazolium acetate (EmimAc) ionic liquid was weighed, 5 g of dry wood pulp was added, and stirred at 80°C to dissolve. After 60 minutes, a uniform transparent solution was formed (wood pulp / EmimAc solution solid content was 5%). 20°C water was used as a coagulation bath to obtain a cellulose hydrogel, which was freeze-dried to show that it had a porous network structure ( Figure 1 , testing instrument: JEOL JSM-6700F), it can be seen that the structure is relatively loose. Then it was washed with water and vacuum dried at 60℃ for 6 hours to obtain a membrane material.
[0048] The tensile strength of the membrane material obtained in Comparative Example 1 was 98.6 MPa, and the elongation at break was 9% ( Figure 2 , Testing instrument: Universal tensile machine Instron 3365, INSTRON). The membrane material is a dense structure before and after tensile fracture ( Figure 3 , testing instrument: JEOL JSM-6700F).
[0049] Example 1
[0050] Use wood pulp as raw material, add 20g of wood pulp into 500mL of water, and disperse by mechanical stirring.
[0051] Then add 80g of 1-ethyl-3-methylimidazolium acetate (EmimAc) ionic liquid and stir to mix evenly. Spread the wood pulp / EmimAc / water mixture and evaporate the water at 60°C. When there is no obvious water evaporation in the mixture, pressurize at 80°C for 3min at 0.5MPa to form a wood pulp / EmimAc solution (the mass ratio of EmimAc to wood pulp is 80:20). 20°C water is used as a coagulation bath to obtain a high-toughness cellulose hydrogel (see Figure 4 , testing instrument: JEOL JSM-6700F). After freeze-drying, it showed a layered overlapping dense structure (see Figure 5 Then, it was washed with water and dried under vacuum at 60°C for 6 hours to obtain a membrane material.
[0052] The tensile strength of the membrane material obtained in Example 1 was 154.9 MPa and the elongation at break was 57.7% (see Figure 6 , testing instrument: universal tensile machine Instron 3365, INSTRON). The membrane material has a layered and dense structure before tensile fracture, and the layered structure is more obvious after tensile fracture (see Figure 7 ).
[0053] Example 2
[0054] Corn stalks were selected as raw materials, and 100 g of corn stalks were lightly treated by stirring them in 1 L of 2% NaOH aqueous solution at 60° C. for 1.5 h.
[0055] Add 20g of treated corn straw into 500mL of water and disperse with mechanical stirring. Add 80g of 1-ethyl-3-methylimidazolium acetate (EmimAc) ionic liquid and stir to mix evenly. Spread the corn straw / EmimAc / water mixture and evaporate the water at 60°C. When there is no obvious evaporation of water in the mixed solution, pressurize at 60°C for 3min at 1.0MPa to form a corn straw / EmimAc solution (the mass ratio of EmimAc to corn straw is 80:20). Use 20°C water as a coagulation bath to obtain corn straw hydrogel. Then wash with water and dry at 60°C for 6 hours to obtain a straw film material ( Figure 8 ).
[0056] The infrared spectrum of the obtained straw film material showed a peak at 1736 cm -1 、1502cm -1 and 798cm -1 The peaks correspond to the peaks of hemicellulose, lignin and SiO2, respectively, indicating that there are multiple components in the obtained straw film ( Fig. 9 , testing instrument: Nicolet6700, Thermo Fisher). The contents of cellulose, hemicellulose and lignin in the straw film were 71.1%, 22.2% and 3.0% respectively.
[0057] The tensile strength of the straw film prepared in Example 2 is 107.4 MPa, the elongation at break is 26.1%, and the toughness is 29.1 MJ / m 3 , which is much higher than commercial cellophane and straw film material prepared by conventional dissolution regeneration method (preparation method see comparative example 1) (see Fig.10 , Testing instrument: Universal tensile machine Instron 3365, INSTRON).
[0058] Example 3
[0059] Wood pulp was selected as the raw material. 15 g of wood pulp was added to 500 mL of water and dispersed by mechanical stirring. Then 85 g of 1-butyl-3-methylimidazolium acetate (BmimAc) ionic liquid was added and stirred to mix evenly. The wood pulp / BmimAc / water mixture was spread and the water was evaporated at 60°C. When there was no obvious evaporation of water in the mixed solution, it was pressurized at 80°C for 3 min under a pressure of 0.5 MPa to form a wood pulp / BmimAc solution (the mass ratio of BmimAc to wood pulp was 85:15). A 0°C BmimAc aqueous solution (BmimAc mass concentration of 50%) was used as a coagulation bath to obtain a high-toughness cellulose hydrogel. It was then washed with water and dried at 60°C for 5 hours to obtain a membrane material.
[0060] The tensile strength of the membrane material obtained in Example 3 is 156.2 MPa, and the elongation at break is 15.5%.
[0061] Example 4
[0062] Cotton pulp was selected as the raw material. 25 g of cotton pulp was added to 500 mL of water and dispersed by mechanical stirring. Then 75 g of 1-butyl-3-methylimidazolium acetate (BmimAc) ionic liquid was added and stirred to mix evenly. The cotton pulp / BmimAc / water mixture was spread and the water was evaporated at 60°C. When there was no obvious evaporation of water in the mixed solution, it was pressurized at 80°C for 3 min under 0.5 MPa pressure to form a cotton pulp / BmimAc solution (the mass ratio of BmimAc to cotton pulp was 75:25). A 0°C BmimAc aqueous solution (BmimAc mass concentration of 30%) was used as a coagulation bath to obtain a high-toughness cellulose hydrogel. It was then washed with water and vacuum dried at 60°C for 4 hours to obtain a membrane material.
[0063] The tensile strength of the membrane material obtained in Example 4 was 141.1 MPa, and the elongation at break was 54.4%.
[0064] Example 5
[0065] Wood pulp was selected as the raw material. 20 g of wood pulp was added to 500 mL of water and dispersed by mechanical stirring. Then 80 g of 1-allyl-3-methylimidazolium chloride (AmimCl) ionic liquid was added and stirred to mix evenly. The wood pulp / AmimCl / water mixture was spread and the water was evaporated at 60°C. When there was no obvious evaporation of water in the mixed solution, pressurized at 80°C for 3 min under 1.0 MPa pressure to form a wood pulp / AmimCl solution (the mass ratio of AmimCl to wood pulp was 80:20). 20°C water was used as a coagulation bath to obtain a high-toughness cellulose hydrogel. Then it was washed with water and vacuum dried at 60°C for 4 hours to obtain a membrane material.
[0066] The tensile strength of the membrane material prepared in Example 5 is 87.8 MPa, and the elongation at break is 24.6%.
[0067] Example 6
[0068] Select poplar wood powder as raw material. 100g poplar wood powder is stirred in 1L of 2% NaOH aqueous solution at 60℃ for 0.5h. Add 20g treated poplar wood powder to 500mL water and disperse it by mechanical stirring. Then add 80g of 1-ethyl-3-methylimidazolium acetate (EmimAc) ionic liquid and stir to mix evenly. Spread the poplar wood powder / EmimAc / water mixture and evaporate the water at 60℃. When there is no obvious water evaporation in the mixed solution, pressurize at 60℃ for 3min under 1.0MPa pressure to form a poplar wood powder / EmimAc solution (the mass ratio of EmimAc to poplar wood powder is 80:20). 20℃ water is used as a coagulation bath to obtain a poplar wood powder hydrogel. Then wash with water and dry at 60℃ for 6 hours to obtain a poplar wood film material.
[0069] The contents of cellulose, hemicellulose and lignin in the poplar film material prepared in Example 6 are 61.5%, 19.5% and 16.8% respectively. The tensile strength of the poplar film is 92.4 MPa, and the elongation at break is 28.2%.
[0070] Example 7
[0071] Pennisetum grass powder was selected as the raw material. 100g of Pennisetum grass powder was stirred in 1L of acetic acid (3mL) / NaClO2 (10g) / water at 60℃ for 1.0h. 20g of treated Pennisetum grass powder was added to 500mL of water and dispersed by mechanical stirring. Then 80g of 1-butyl-3-methylimidazolium acetate (BmimAc) ionic liquid was added and stirred to mix evenly. The grass powder / BmimAc / water mixture was spread and the water was evaporated at 60℃. When there was no obvious water evaporation in the mixed solution, it was pressurized at 60℃ for 3min under 1.0MPa pressure to form a grass powder / BmimAc solution (the mass ratio of BmimAc to grass powder was 80:20). 20℃ water was used as a coagulation bath to obtain a grass powder hydrogel. Then it was washed with water and dried at 60℃ for 6 hours to obtain a grass powder film material.
[0072] The contents of cellulose, hemicellulose and lignin in the obtained grass powder film material are 64.0%, 20.5% and 6.3% respectively. The tensile strength of the straw film is 96.6MPa and the elongation at break is 30.2%.
[0073] Example 8
[0074] Chitosan was selected as the raw material. 20 g of chitosan was added to 500 mL of water and dispersed by mechanical stirring. Then 80 g of 1-butyl-3-methylimidazolium acetate (BmimAc) ionic liquid was added and stirred to mix evenly. The chitosan / BmimAc / water mixture was spread and the water was evaporated at 60°C. When there was no obvious evaporation of water in the mixed solution, it was pressurized at 60°C for 3 min under a pressure of 1.0 MPa to form a chitosan / BmimAc solution (the mass ratio of BmimAc to chitosan was 80:20). 20°C water was used as a coagulation bath to obtain a chitosan hydrogel. Then it was washed with water and dried at 60°C for 5 hours to obtain a chitosan film material.
[0075] The tensile strength of the obtained chitosan film material is 89.2 MPa, and the elongation at break is 20.1%.
[0076] The above is an explanation of the embodiments of the present invention. However, the present invention is not limited to the above embodiments. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a biomass material, characterized in that: The steps include: Step 1: mixing the biomass with or without light treatment with water to obtain a biomass dispersion; Step 2: Add ionic liquid to the biomass dispersion and stir to mix evenly; Step 3: heating and dehydrating the biomass / water / ionic liquid mixture until no obvious water evaporates from the mixture, applying pressure; Step 4: placing the material obtained in step 3 in a coagulation bath for coagulation to obtain a biomass gel; Step 5: Gel the biomass, wash and dry.
2. The preparation method according to claim 1, characterized in that: The biomass is selected from the group consisting of films, fibers, and boards. Preferably, the biomass is selected from plant straw, grass plants, various wood chips, and agricultural and forestry wastes. For example, one or more of cellulose, chitosan, starch, chitin, wheat straw, corn straw, cotton straw, Chinese medicine residues, foxtail grass, pennisetum, barnyard grass, reed, corn cob, bagasse, fruit shells, plant stems and leaves, waste wood chips, wood powder, sawdust, and bamboo powder. Preferably, the cellulose is selected from one or more of microcrystalline cellulose, cotton pulp, refined cotton, defatted cotton, wood pulp, cotton linter, bamboo pulp, straw pulp and bacterial cellulose.
3. The preparation method according to claim 1, characterized in that: The light treatment is at least one of an alkaline solution treatment, a peracetic acid aqueous solution treatment, a p-toluenesulfonic acid aqueous solution treatment, and an acetic acid / NaClO2 aqueous solution treatment method.
4. The preparation method according to claim 1, characterized in that: In the step 1, the biomass and water are mixed by stirring or beating to prepare a biomass water dispersion. Preferably, the ratio of biomass to water is 1% to 30%, preferably 3% to 20%.
5. The preparation method according to claim 1, characterized in that: The ionic liquid is a molten salt formed by substituted or unsubstituted imidazole or pyridinium cations and anions with a melting point below 100°C; Preferably, the substituent on the imidazole or pyridinium cation is C 1-6 Alkyl, C 1-6 The anion is at least one of an alkyl acid ion, a halide ion, and an organic phosphate ion. For example, the ionic liquid is selected from at least one of 1-allyl-3-methylimidazolium chloride, 1-butyl-3-methylimidazolium acetate ionic liquid and 1-ethyl-3-methylimidazolium acetate.
6. The preparation method according to claim 1, characterized in that: The mass ratio of the ionic liquid to the biomass is 13:7 to 17:3, preferably 7:3 to 8:2, for example, 3:1, 3.1:1, 3.2:1, 3.3:1, 3.4:1, 3.5:1, 3.6:1, 3.7:1, 3.8:1, 3.9:1, 4.0:1 and any range or ratio between the above arbitrary point values.
7. The preparation method according to claim 1, characterized in that: The temperature of heating and dehydration in step 3 is 60-110°C, preferably 80-110°C, for example, 80°C, 85°C, 90°C, 95°C, 100°C, 105°C, 110°C and any range or ratio between the above-mentioned arbitrary point values. Preferably, step 3 comprises pressurizing at 0.5 MPa to 5 MPa for 3 min at 80 to 110° C., for example, pressurizing at 0.5 MPa for 3 min at 80° C.
8. The preparation method according to claim 1, characterized in that: The coagulation bath is any one of water, alcohol, a mixture of water and an ionic liquid, and a mixture of an alcohol and an ionic liquid; For example, the alcohol is selected from at least one of ethanol, methanol, isopropanol, n-propanol and n-butanol; Preferably, when the coagulation bath is a mixture of water and an ionic liquid, the mass ratio of water to the ionic liquid in the mixture is 1:(0.1-4). For example, 1:0.1, 1:0.15, 1:0.2, 1:0.25, 1:0.3, 1:0.35, 1:0.4, 1:0.45, 1:0.5, 1:0.55, 1:0.6, 1:0.65, 1:0.67, 1:1, 1:1.5, 1:2, 1:2.5, 1:3, 1:3.5, 1:4 or the range between any two of the above values. Preferably, when the coagulation bath is a mixture of alcohol and ionic liquid, the mass ratio of the alcohol to the ionic liquid in the mixture is 1:(0.1-4). For example, 1:0.1, 1:0.15, 1:0.2, 1:0.25, 1:0.3, 1:0.35, 1:0.4, 1:0.45, 1:0.5, 1:0.55, 1:0.6, 1:0.65, 1:0.67, 1:1, 1:1.5, 1:2, 1:2.5, 1:3, 1:3.5, 1:4 or the range between any two of the above values.
9. The preparation method according to any one of claims 1 to 8, characterized in that: The temperature of the coagulation bath can be 0°C to 50°C, preferably 0°C to 40°C, for example 0°C, 5°C, 10°C, 15°C, 20°C, 25°C, 30°C, 35°C, 40°C or a range between any two of the above values.
10. A biomass material, characterized in that: The biomass material is obtained by the preparation method of the biomass material according to any one of claims 1 to 9. Preferably, the elongation at break of the biomass material exceeds 15%.
Citation Information
Cited By
Whole-plant high-toughness plastic material as well as preparation method and application thereof
CN119392526A
A kind of whole plant high toughness plastic material and its preparation method and application
CN119392526B