High-toughness polylactic acid heat shrink film as well as preparation method and application thereof

By employing biaxial stretching technology and toughening agents, the problems of uneven shrinkage and easy breakage in the longitudinal direction of heat-shrinkable polylactic acid (PLA) films have been solved, resulting in a high-toughness and uniformly shrinkable PLA heat-shrinkable film suitable for packaging materials.

CN118909284APending Publication Date: 2024-11-08SHANDONG SHENGHE PLASTIC DEV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411148989.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing heat-shrinkable polylactic acid films have uneven shrinkage in the unstretched direction, are prone to breakage under high temperature and humidity, are brittle, and are difficult to control effectively in the longitudinal direction.

Method used

A high-toughness polylactic acid heat-shrinkable film is prepared by using a biaxial stretching process, combining amorphous and crystalline polylactic acid, adding toughening agents such as polypropylene carbonate-grafted polyurethane elastomer, reserving a 10% pre-shrinkage width in the transverse direction, and performing water bath shrinkage treatment at high temperature.

Benefits of technology

It improves the longitudinal elongation at break, ensuring that the membrane is not easily broken under normal temperature and humidity conditions as well as high temperature and high humidity conditions, and has good toughness and shrinkage uniformity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005003059420000051
    Figure BDA0005003059420000051
  • Figure BDA0005003059420000052
    Figure BDA0005003059420000052
  • Figure BDA0005003059420000071
    Figure BDA0005003059420000071
Patent Text Reader

Abstract

The invention relates to a high-toughness polylactic acid heat shrink film as well as a preparation method and application thereof, and belongs to the field of heat shrink films. The heat-shrinkable polylactic acid film is processed for 10 seconds at the temperature of 90 DEG C, the shrinkage rate in the transverse direction (TD) is larger than or equal to 40%, the shrinkage rate in the longitudinal direction (MD) ranges from 1% to 20%, and when the shrinkage rate in the transverse direction ranges from 40% to 70%, the longitudinal elongation at break is larger than or equal to 180% after the heat-shrinkable polylactic acid film is placed at the normal temperature and the normal humidity (the temperature is smaller than or equal to 30 DEG C, and the humidity is smaller than or equal to 60%) for 4 months; when the transverse shrinkage rate is greater than or equal to 70%, the longitudinal elongation at break is greater than or equal to 180% after being placed at normal temperature and normal humidity (the temperature is less than or equal to 30 DEG C, and the humidity is less than or equal to 60%) for 6 months. The polylactic acid thermal shrinkage film has high longitudinal elongation at break when placed at normal temperature and normal humidity and placed at high temperature and high humidity, and further has the advantages of being not easy to break and good in toughness. The polylactic acid thermal shrinkage film can be directly coated on the surface of a container or coated on the surface of the container after being shrunk at 60-150 DEG C after being subjected to pattern printing, and still has higher longitudinal elongation at break.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a high-toughness polylactic acid heat shrinkable film and a preparation method and application thereof, belonging to the field of heat shrinkable films. Background Art

[0002] Heat shrink film refers to a special material that has a certain shrinkage ability when heated at a predetermined temperature. Heat shrink film is mainly used for identification (labels) and cluster packaging of new products such as beverages, detergents, electronic products, industrial products and fast food. It has the characteristics of bright gloss and close-fitting packaging, and can redefine beverage brands when used. Its gloss and shrinkage can make the packaging pattern on bottled beverages more vivid. The use of shrink film can achieve 360° label design, highlighting the image on supermarket shelves.

[0003] Polylactic acid (PLA) is the most important biodegradable and environmentally friendly polymer material among aliphatic polylactic acids. First of all, PLA materials are bio-based materials. Its monomer raw material lactic acid can be produced on a large scale by fermenting crops such as cassava, straw, Jerusalem artichoke, corn, and biomass waste, so it can completely get rid of dependence on petroleum resources; secondly, PLA materials have excellent biodegradability. Under natural composting conditions, it can be completely degraded into carbon dioxide and water in 2-3 months, which is harmless to the environment and can achieve recyclable and renewable resource utilization. Polylactic acid has become a new direction for solving the "white pollution problem". The use of polylactic acid materials to process biaxially oriented polylactic acid heat shrinkable film is of great significance to environmental protection and the development of the plastics industry.

[0004] Since the heat-shrinkable polylactic acid film requires a larger shrinkage rate in the transverse direction, the heat-shrinkable polylactic acid film production lines at home and abroad currently adopt a unidirectional stretching process, that is, generally only transverse stretching is adopted, including preheating, stretching, heat setting and cooling areas. Since only unidirectional stretching is performed, or the stretching ratio in the longitudinal direction is very small, the performance of the product in the unstretched direction is difficult to be effectively controlled, which will lead to uneven shrinkage in the unstretched direction. Moreover, at room temperature, especially after being placed under high temperature and high humidity for a period of time, the shrink film will suddenly decrease its elongation at break along the MD direction, and even appear in single digits, which shows that it is very easy to break and brittle. Summary of the invention

[0005] To achieve the above object, the present invention provides the following technical solutions:

[0006] A high-toughness polylactic acid heat-shrinkable film and a preparation method and application thereof, wherein the heat-shrinkable polylactic acid film is treated at 90°C for 10 seconds, has a shrinkage rate of ≥40% in the transverse direction (TD) and a shrinkage rate of -1% to 20% in the longitudinal direction (MD), and when the shrinkage rate in the transverse direction is 40-70%, after being placed at room temperature and humidity (temperature ≤30°C, humidity ≤60%) for 4 months, the longitudinal elongation at break is ≥180%; when the shrinkage rate in the transverse direction is ≥70%, after being placed at room temperature and humidity (temperature ≤30°C, humidity ≤60%) for 6 months, the longitudinal elongation at break is ≥180%;

[0007] The high-toughness polylactic acid heat shrinkable film fixes the sample in the transverse direction, reserves 10% of the pre-shrinkage width in the transverse direction, performs water bath shrinkage, and after being treated at 90°C for 10 seconds, the longitudinal elongation at break is ≥100%; the method for fixing the sample in the transverse direction of the high-toughness polylactic acid heat shrinkable film includes a self-made rectangular clamp, which is divided into a rectangular clamp lower plate, hollowed in the middle, and with a frame width of 1-5cm. Another rectangular clamp upper plate is the same size as the lower plate, hollowed in the middle, with a frame thickness of 1-5cm, and holes are punched at the same position on the opposite sides of the upper and lower plates of the clamp for bolt fixing, and two layers of silicone gaskets are added between the upper and lower plates of the clamp to increase the friction between the film and the metal clamp, as well as a handle fixed on the clamp to facilitate the water bath shrinkage operation. The distance between the opposite sides of the rectangular bolt fixing is measured as X. The original width of the sample when the pre-shrinkage width of 10% is reserved in the transverse direction is Y=X / 90%.

[0008] The mass percentage of the formula is:

[0009] Resin 85-98.9%;

[0010] Toughening resin 1-10%;

[0011] Opening lubricant 0.1-5%;

[0012] The resin raw material comprises amorphous polylactic acid and optional crystalline polylactic acid, wherein the mass fraction of the amorphous polylactic acid is 70-100% of the total resin raw material, and the mass fraction of the crystalline polylactic acid is 0-30% of the total resin raw material; wherein the amount of the crystalline polylactic acid used depends on the degree of crystallization of the amorphous polylactic acid and the required shrinkage rate to meet the aesthetic requirements of the shrink packaging of the final product.

[0013] The preparation method is:

[0014] (1) Batching: Various polylactic acid raw materials are measured according to the raw material ratio and then enter the inlet of each extruder.

[0015] (2) Extruded sheet: The melt extruded by the extruder enters the die through respective filters, metering pumps, etc. to extrude the melt into a sheet, and then cools on the casting roll to form an unstretched sheet.

[0016] (3) Unstretched sheet: After preheating at 10-50°C above the softening point, the film is stretched 1.0-1.5 times in the longitudinal direction and then stretched 5.0-5.5 times in the transverse direction. The transverse stretching temperature is 3-10°C higher than the longitudinal stretching temperature. The stretched film is cold-set and then pulled and rolled or corona treated to obtain a semi-finished film.

[0017] Preferably, the high-toughness polylactic acid heat shrinkable film can be a single-layer structure or a multi-layer structure of two or more layers. When it has a structure of two or more layers, the polylactic acid film can be divided into a polylactic acid core layer or a polylactic acid surface layer, wherein the thickness of the polylactic acid surface layer is 5-20% of the total thickness.

[0018] Preferably, the high-toughness polylactic acid heat shrinkable film has a thickness of 20-100 μm.

[0019] Preferably, the high-toughness polylactic acid heat shrinkable film has a thickness of 30-60 μm.

[0020] Preferably, the amorphous polylactic acid and the crystalline polylactic acid are both polylactic acids obtained by polymerizing L-type and D-type lactic acid monomers, and the total content of L-type and D-type lactic acid monomers is calculated as 100 mol%;

[0021] In the amorphous polylactic acid, the molar content of L-type polylactic acid is 85-97%, and the molar content of D-type polylactic acid is 3-15%. Polylactic acids of different chirality can significantly reduce the crystallinity of polylactic acid.

[0022] In the crystalline polylactic acid, the molar content of L-type polylactic acid is 97-100%, and the molar content of D-type polylactic acid is 0-3%, or the molar content of L-type polylactic acid is 0-3%, and the molar content of D-type polylactic acid is 97-100%.

[0023] Preferably, the slippery opening agent is one or more of silicon dioxide, mica powder, alumina, kaolin or paraffin; wherein the particle size of silicon dioxide is ≤4um;

[0024] Preferably, the double-layer or more multi-layer structure has two polylactic acid surface layers, at least one of the polylactic acid surface layers contains a slippery opening agent, and the amount of the slippery opening agent is 0.1%-5% of the total amount of the polylactic acid surface layer.

[0025] Preferably, the toughening resin is polypropylene carbonate grafted polyurethane elastomer (PPCU) or propylene carbonate-phthalate copolymer (PPC-P).

[0026] Preferably, the high-toughness polylactic acid heat shrinkable film can be directly or after pattern printing, and then shrink-labeled at 60-150° C., and can be heated by water vapor, hot air and infrared.

[0027] Since the added polypropylene carbonate (PPC) is a biodegradable aliphatic polyester prepared by copolymerization of greenhouse gas carbon dioxide (CO2) and propylene oxide under catalyst, certain temperature and pressure conditions. Polypropylene carbonate (PPC) and polylactic acid have good compatibility, the modified polypropylene carbonate grafted polyurethane elastomer (PPCU), propylene carbonate-phthalate copolymer (PPC-P) firstly has good toughness itself, secondly further reduces the crystallization ability of polylactic acid resin, and thirdly produces irregular entanglement of molecular chains in the direction that is not effectively stretched, thereby achieving a period of significantly improving the elongation at break of the shrink film along the MD direction, and achieving high toughness product performance.

[0028] Various additives can be added to the formula as needed, such as waxes, antioxidants, antistatic agents, nucleating agents, viscosity reducers, tackifiers, chain extenders, heat stabilizers, coloring pigments, anti-coloring agents, anti-ultraviolet absorbers, etc.

[0029] The beneficial effects of the present invention are:

[0030] The polylactic acid heat shrinkable film obtained by the invention has a higher longitudinal elongation at break when placed at normal temperature and humidity or at high temperature and high humidity, and is thus not easy to break and has good toughness.

[0031] The present invention also provides a method for preparing a high-toughness polylactic acid heat shrinkable film. The polylactic acid heat shrinkable film can be directly or after pattern printing, and then shrunk and coated on the surface of a container under the condition of 60-150° C., and still has a high longitudinal elongation at break. DETAILED DESCRIPTION

[0032] Example 1

[0033] A high-toughness polylactic acid heat shrinkable film and a preparation method and application thereof, wherein the formula (mass percentage) is:

[0034] Resin 98.9%;

[0035] Propylene carbonate-phthalate copolymer 1%;

[0036] Mica powder 0.1%;

[0037] The mass fraction of amorphous polylactic acid accounts for 70% of the total resin raw materials, and the mass fraction of crystalline polylactic acid accounts for 30% of the total resin raw materials;

[0038] In the amorphous polylactic acid, the molar content of L-type polylactic acid is 85-97%, and the molar content of D-type polylactic acid is 3-15%. Polylactic acids of different chirality can significantly reduce the crystallinity of polylactic acid.

[0039] In the crystalline polylactic acid, the molar content of L-type polylactic acid is 97-100%, and the molar content of D-type polylactic acid is 0-3%, or the molar content of L-type polylactic acid is 0-3%, and the molar content of D-type polylactic acid is 97-100%.

[0040] The preparation method is:

[0041] (1) Batching: Various polylactic acid raw materials are measured according to the raw material ratio and then enter the inlet of each extruder.

[0042] (2) Extruded sheet: The melt extruded by the extruder enters the die through respective filters, metering pumps, etc. to extrude the melt into a sheet, and then cools on the casting roll to form an unstretched sheet.

[0043] (3) Unstretched sheet: After preheating at 50°C above the softening point, the film is stretched 1.5 times in the longitudinal direction and then 5.5 times in the transverse direction. The transverse stretching temperature is 10°C higher than the longitudinal stretching temperature. The stretched film is cold-set and then pulled and rolled or corona treated to obtain a semi-finished film.

[0044] Method for fixing the sample of high-toughness polylactic acid heat shrinkable film in the transverse direction: measure the distance between the opposite sides of the rectangular bolts as X. When a 10% pre-shrinkage width is reserved in the transverse direction, the original width of the sample is Y=X / 90%.

[0045] The obtained high-toughness polylactic acid heat shrinkable film has a thickness of 20 μm and a single-layer structure.

[0046] Example 2

[0047] A high-toughness polylactic acid heat shrinkable film and a preparation method and application thereof, wherein the formula (mass percentage) is:

[0048] Resin 85%;

[0049] Polypropylene carbonate grafted polyurethane elastomer 10%;

[0050] Silicon dioxide (particle size 4um) 5%;

[0051] The mass fraction of amorphous polylactic acid accounts for 100% of the total resin raw materials, and the mass fraction of crystalline polylactic acid accounts for 0% of the total resin raw materials;

[0052] In the amorphous polylactic acid, the molar content of L-type polylactic acid is 85-97%, and the molar content of D-type polylactic acid is 3-15%. Polylactic acids of different chirality can significantly reduce the crystallinity of polylactic acid.

[0053] The preparation method is:

[0054] (1) Batching: Various polylactic acid raw materials are measured according to the raw material ratio and then enter the inlet of each extruder.

[0055] (2) Extruded sheet: The melt extruded by the extruder enters the die through respective filters, metering pumps, etc. to extrude the melt into a sheet, and then cools on the casting roll to form an unstretched sheet.

[0056] (3) Unstretched sheet: After preheating at 30°C above the softening point, the film is stretched 1.5 times in the longitudinal direction and then stretched 5.0 times in the transverse direction. The transverse stretching temperature is 7°C higher than the longitudinal stretching temperature. The stretched film is cold-set and then pulled and rolled or corona treated to obtain a semi-finished film.

[0057] Method for fixing the sample of high-toughness polylactic acid heat shrinkable film in the transverse direction: measure the distance between the opposite sides of the rectangular bolts as X. When a 10% pre-shrinkage width is reserved in the transverse direction, the original width of the sample is Y=X / 90%.

[0058] The obtained high-toughness polylactic acid heat shrinkable film has a thickness of 80 μm and a double-layer structure.

[0059] Example 3

[0060] A high-toughness polylactic acid heat shrinkable film and a preparation method and application thereof, wherein the formula (mass percentage) is:

[0061]

[0062] The mass fraction of amorphous polylactic acid accounts for 70-100% of the total resin raw materials, and the mass fraction of crystalline polylactic acid accounts for 0-30% of the total resin raw materials;

[0063] In the amorphous polylactic acid, the molar content of L-type polylactic acid is 85-97%, and the molar content of D-type polylactic acid is 3-15%. Polylactic acids of different chirality can significantly reduce the crystallinity of polylactic acid.

[0064] In the crystalline polylactic acid, the molar content of L-type polylactic acid is 97-100%, and the molar content of D-type polylactic acid is 0-3%, or the molar content of L-type polylactic acid is 0-3%, and the molar content of D-type polylactic acid is 97-100%.

[0065] The preparation method is:

[0066] (1) Batching: Various polylactic acid raw materials are measured according to the raw material ratio and then enter the inlet of each extruder.

[0067] (2) Extruded sheet: The melt extruded by the extruder enters the die through respective filters, metering pumps, etc. to extrude the melt into a sheet, and then cools on the casting roll to form an unstretched sheet.

[0068] (3) Unstretched sheet: After preheating at 10°C above the softening point, the film is stretched 1.0 times in the longitudinal direction and then 5.0 times in the transverse direction. The transverse stretching temperature is 3°C higher than the longitudinal stretching temperature. The stretched film is cold-set and then pulled and rolled or corona treated to obtain a semi-finished film.

[0069] Method for fixing the sample of high-toughness polylactic acid heat shrinkable film in the transverse direction: measure the distance between the opposite sides of the rectangular bolts as X. When a 10% pre-shrinkage width is reserved in the transverse direction, the original width of the sample is Y=X / 90%.

[0070] The obtained high-toughness polylactic acid heat shrinkable film has a thickness of 100 μm and a three-layer structure.

[0071] Example 4

[0072] A high-toughness polylactic acid heat shrinkable film and a preparation method and application thereof, wherein the formula (mass percentage) is:

[0073]

[0074] The mass fraction of amorphous polylactic acid accounts for 70-100% of the total resin raw materials, and the mass fraction of crystalline polylactic acid accounts for 0-30% of the total resin raw materials;

[0075] In the amorphous polylactic acid, the molar content of L-type polylactic acid is 85-97%, and the molar content of D-type polylactic acid is 3-15%. Polylactic acids of different chirality can significantly reduce the crystallinity of polylactic acid.

[0076] In the crystalline polylactic acid, the molar content of L-type polylactic acid is 97-100%, and the molar content of D-type polylactic acid is 0-3%, or the molar content of L-type polylactic acid is 0-3%, and the molar content of D-type polylactic acid is 97-100%.

[0077] The preparation method is:

[0078] (1) Batching: Various polylactic acid raw materials are measured according to the raw material ratio and then enter the inlet of each extruder.

[0079] (2) Extruded sheet: The melt extruded by the extruder enters the die through respective filters, metering pumps, etc. to extrude the melt into a sheet, and then cools on the casting roll to form an unstretched sheet.

[0080] (3) Unstretched sheet: After preheating at 30°C above the softening point, the film is stretched 1.2 times in the longitudinal direction and then stretched 5.3 times in the transverse direction. The transverse stretching temperature is 7°C higher than the longitudinal stretching temperature. The stretched film is cold-set and then pulled and rolled or corona treated to obtain a semi-finished film.

[0081] Method for fixing the sample of high-toughness polylactic acid heat shrinkable film in the transverse direction: measure the distance between the opposite sides of the rectangular bolts as X. When a 10% pre-shrinkage width is reserved in the transverse direction, the original width of the sample is Y=X / 90%.

[0082] The obtained high-toughness polylactic acid heat shrinkable film has a thickness of 40 μm and a double-layer structure.

[0083]

[0084] Table 1 Performance test table of embodiments and comparative examples

[0085] project unit Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Longitudinal elongation at break (1 month) % 225 228 204 235 6 Transverse elongation at break (1 month) % 88 82 80 87 75 Longitudinal elongation at break (2 months) % 221 225 202 205 4 Transverse elongation at break (2 months) % 82 82 75 75 75 Longitudinal elongation at break (3 months) % 218 223 201 195 4 Transverse elongation at break (3 months) % 80 81 74 72 72 Longitudinal elongation at break (4 months) % 216 215 195 187 5 Transverse elongation at break (4 months) % 75 77 72 70 71 Longitudinal elongation at break (May) % 208 192 190 5 4 Transverse elongation at break (May) % 72 75 70 68 68 Longitudinal elongation at break (6 months) % 195 185 186 4 4 Transverse elongation at break (June) % 72 75 68 65 65

[0086] Table 2 The longitudinal and transverse elongation at break of each embodiment and comparative example over time

[0087] It can be seen from Tables 1 and 2 that the properties of the polylactic acid heat shrinkable film obtained in the present invention are similar to those of commercially available polylactic acid heat shrinkable films, and have a higher longitudinal elongation at break when placed at room temperature and humidity and at high temperature and humidity, and are thus not easy to break and have good toughness.

[0088] The polylactic acid heat shrinkable film obtained by the present invention can be directly or after pattern printing, and then covered on the surface of a container after shrinkage at 60-150° C., and still has a relatively high longitudinal elongation at break.

Claims

1. A high-toughness polylactic acid heat shrinkable film and its preparation method and application, It is characterized in that The heat-shrinkable polylactic acid film is treated at 90° C. for 10 seconds, and has a shrinkage rate of ≥40% in the transverse direction and a shrinkage rate of -1% to 20% in the longitudinal direction; and when the shrinkage rate in the transverse direction is 40-70%, after being placed at room temperature and humidity for 4 months, the longitudinal elongation at break is ≥180%; when the shrinkage rate in the transverse direction is ≥70%, after being placed at room temperature and humidity for 6 months, the longitudinal elongation at break is ≥180%; The normal temperature and humidity conditions are: temperature ≤ 30°C, humidity ≤ 60%; The high-toughness polylactic acid heat shrinkable film is fixed along the transverse direction, and a 10% pre-shrinkage width is reserved in the transverse direction. The film is shrunk in a water bath, and after being treated at 90° C. for 10 seconds, the longitudinal elongation at break is ≥100%; The mass percentage of the formula is: Resin raw material 85-98.9%; Toughening resin 1-10%; Opening lubricant 0.1-5%; The resin raw material comprises amorphous polylactic acid and optional crystalline polylactic acid, the mass fraction of the amorphous polylactic acid accounts for 70-100% of the total resin raw material, and the mass fraction of the crystalline polylactic acid accounts for 0-30% of the total resin raw material; The preparation method is: (1) Batching: Various polylactic acid raw materials are measured according to the raw material ratio and then enter the inlet of each extruder. (2) Extruded sheet: The melt extruded by the extruder enters the die through respective filters, metering pumps, etc. to extrude the melt into a sheet, and then cools on the casting roll to form an unstretched sheet. (3) Unstretched sheet: After preheating at 10-50°C above the softening point, the film is stretched 1.0-1.5 times in the longitudinal direction and then stretched 5.0-5.5 times in the transverse direction. The transverse stretching temperature is 3-10°C higher than the longitudinal stretching temperature. The stretched film is cold-set and then pulled and rolled or corona treated to obtain a semi-finished film.

2. A high-toughness polylactic acid heat shrinkable film and a preparation method and application thereof according to claim 1, It is characterized in that The high-toughness polylactic acid heat shrinkable film can have a single-layer structure or a multi-layer structure of two or more layers. When it has a structure of two or more layers, the polylactic acid film can be divided into a polylactic acid core layer or a polylactic acid surface layer, wherein the thickness of the polylactic acid surface layer is 5-20% of the total thickness.

3. A high-toughness polylactic acid heat shrinkable film and a preparation method and application thereof according to claim 1, It is characterized in that The high-toughness polylactic acid heat shrinkable film has a thickness of 20-100 μm.

4. A high-toughness polylactic acid heat shrinkable film and a preparation method and application thereof according to claim 4, It is characterized in that The high-toughness polylactic acid heat shrinkable film has a thickness of 30-60 μm.

5. A high-toughness polylactic acid heat shrinkable film and a preparation method and application thereof according to claim 1, It is characterized in that The amorphous polylactic acid and the crystalline polylactic acid are both polylactic acids obtained by polymerizing L-type and D-type lactic acid monomers, and the total content of L-type and D-type lactic acid monomers is calculated as 100 mol%; In the amorphous polylactic acid, the molar content of L-type polylactic acid is 85-97%, and the molar content of D-type polylactic acid is 3-15%. Polylactic acids of different chirality can significantly reduce the crystallinity of polylactic acid. In the crystalline polylactic acid, the molar content of L-type polylactic acid is 97-100%, and the molar content of D-type polylactic acid is 0-3%, or the molar content of L-type polylactic acid is 0-3%, and the molar content of D-type polylactic acid is 97-100%.

6. A high-toughness polylactic acid heat shrinkable film and a preparation method and application thereof according to claim 1, It is characterized in that The smooth opening agent is one or more of silicon dioxide, mica powder, aluminum oxide, kaolin or paraffin; wherein the particle size of silicon dioxide is ≤4um.

7. A high-toughness polylactic acid heat shrinkable film and a preparation method and application thereof according to claim 2, It is characterized in that The double-layer or more multi-layer structure has two polylactic acid surface layers, at least one of which contains a smooth opening agent, and the amount of the smooth opening agent is 0.1%-5% of the total amount of the polylactic acid surface layer.

8. A high-toughness polylactic acid heat shrinkable film and a preparation method and application thereof according to claim 1, It is characterized in that The toughening resin is polypropylene carbonate grafted polyurethane elastomer or propylene carbonate-phthalate copolymer.

9. A high-toughness polylactic acid heat shrinkable film according to claims 1-8, and a preparation method and application thereof, It is characterized in that The high-toughness polylactic acid heat shrinkable film can be directly or after pattern printing, and can be shrunk at 60-150° C., and can be heated by water vapor, hot air and infrared.