PVC (polyvinyl chloride) coiled material with static electricity conducting function and preparation process thereof

By using electrocarbon black and metal powder as conductive fillers in PVC coils and coating conductive coatings during the extrusion process to form a conductive network, the problem of low conductivity of PVC coils is solved, and the electrostatic conduction effect is significantly improved and Security.

CN118909290AInactive Publication Date: 2024-11-08JIANGSU KA LAI NEW DECORATIVE MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411239711.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The current PVC coils have low conductivity, resulting in poor electrostatic conduction effect and reduced safety.

Method used

Electric carbon black and metal powder are used as conductive fillers, combined with polyvinyl chloride resin for mixing, and coated with conductive coating during the extrusion process to form a continuous conductive network to improve the electrostatic conductivity.

Benefits of technology

It significantly improves the conductivity and electrostatic conduction effect of PVC coils, and improves safety and wear resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118909290A_ABST
    Figure CN118909290A_ABST
Patent Text Reader

Abstract

The invention discloses a PVC coiled material with a static conductive function and a preparation process thereof, and relates to the technical field of PVC coiled materials, raw materials formed after mixing are installed and put into an extruder to be extruded, the extrusion pressure of the extruder ranges from 0.022 MPa to 0.45 MPa, the extrusion speed ranges from 2 m / min to 3 m / min, the extruded raw material is a coiled material A, the extruded raw material is a PVC coiled material B, the PVC coiled material B is a PVC coiled material C, and the PVC coiled material B is a PVC coiled material B; the surface of the coiled material A is coated with a conductive coating in the extrusion process of the coiled material A, the conductive coating forms a continuous conductive network to improve the static conductivity of the coiled material A, the conductive network is latticed, the surface of the coiled material A is coated with the conductive coating to form a coiled material C, and the conductive coating is formed by mixing the following materials in parts by weight: 27 parts of graphite, 13 parts of graphite fibers, 16 parts of carbon fibers, 12 parts of graphene and 160 parts of water. And stirring is performed at the temperature of 56 DEG C for 12 minutes, so that the electric conductivity of the PVC coiled material is improved, the static conductive effect of the PVC coiled material is greatly improved, and the safety is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of PVC coiled materials, in particular to a PVC coiled material with a static electricity conductive function and a preparation process thereof. Background Art

[0002] The background technology of PVC coils with electrostatic conductivity is mainly based on the electrostatic dissipation performance of conductive PVC materials, which can effectively eliminate the harm caused by static electricity and protect equipment from damage caused by electrostatic discharge. Conductive PVC materials achieve the electrostatic conductivity function through their internal conductive network, so that the charge can be quickly dispersed inside the material, thereby preventing static electricity accumulation. However, the conductivity of existing PVC coils is not high, which makes the electrostatic conductivity of PVC coils poor and reduces safety.

[0003] The defects of existing PVC coils are: 1. Patent document CN211198048U discloses a guide device for conveying PVC antistatic coiled materials, "including two symmetrically arranged mounting frames, the left and right ends and the middle upper end of the inner side surface of the mounting frame are provided with fixed shafts, the side surface of the fixed shaft is rotatably provided with a first roller, the side surface of the mounting frame is provided with two slide grooves cross-distributed with the fixed shaft, the inner sliding surface of the slide groove is provided with a correction member, the correction member includes an adjustment rod that can move axially along the fixed shaft, the adjustment rod is located between the two mounting frames and is rotatably provided with a second roller, and the second roller is provided with an annular baffle at one end close to the mounting frame. The guide device for conveying PVC antistatic coiled materials is easy to install and can be adjusted. It can position and guide coils of different sizes, which is convenient for conveying coiled materials, and the tightness of the coiled materials during conveying can be adjusted, which is convenient for the winding operation of the coiled materials and easy to use", but the low conductivity of the existing PVC coiled materials makes the electrostatic conduction effect of the PVC coiled materials poor and reduces the safety; 2. Patent document CN101787788B discloses a process and complete set of equipment for manufacturing anti-static PVC coiled materials with uniformly distributed conductive screens inside the material. "The method is provided with a molding process, a lamination process, a cutting process, a polishing process, a splicing process and a finishing process after the drying process. The surface of the PVC coiled material spliced ​​by the above method is beautiful and has uniform electrostatic conductivity." However, the conductivity of the existing PVC coiled materials is not high, so the electrostatic conductivity effect of the PVC coiled materials is poor and the safety is reduced; 3. Patent document CN102873809B discloses a preparation process of an anti-static PVC homogeneous core-permeable coil floor, "having the following steps: preparing PVC particles through a PVC granulation process; coating the surface of the PVC particles with a conductive slurry, and drying it to form a conductive film on the surface of the PVC particles; or uniformly mixing the conductor in the PVC particles; putting the PVC particles wrapped with the conductive film or the PVC particles mixed with the conductor into a drum vulcanizer for vulcanization and molding; post-processing. The beneficial effects of the present invention are: simple production process, better stability, longer service life of the floor, uniform conductivity, fewer joints during laying, the size can generally reach 2.0 meters × 50 meters, or longer, the pattern is clearer and more natural, and the three-dimensional sense is stronger", but the conductivity of the existing PVC coil is not high, which makes the PVC coil have a poor static conductive effect and reduced safety; 4. Patent document N115895043B discloses a nanoparticle fluid, an antistatic PVC waterproofing membrane and a preparation method. "The nanoparticle fluid includes nanoparticles grafted with organosilicon quaternary ammonium salts, the nanoparticles grafted with organosilicon quaternary ammonium salts are loaded with nanosilver particles, and the nanoparticle fluid is obtained by reacting nanoparticles, organosilicon quaternary ammonium salts and silver salt solutions. The present application adopts a chemical synthesis method to connect nanoparticles, organosilicon quaternary ammonium salt grafts and nanosilver particles together through chemical bonds to obtain a nanoparticle fluid with good conductive effect, which can be used as a new functional additive in the PVC waterproofing membrane formula system and obtain a good antistatic modification effect." However, the conductivity of the existing PVC membrane is not high, which makes the PVC membrane's static conductive effect poor and reduces its safety. Summary of the invention

[0004] The purpose of the present invention is to provide a PVC coil with electrostatic conductivity and a preparation process thereof, so as to solve the technical problem raised in the above background technology that the conductivity of the existing PVC coil is not high, resulting in poor electrostatic conductivity and reduced safety of the PVC coil.

[0005] To achieve the above object, the present invention provides the following technical solution: a process for preparing a PVC coil with a static conductive function, comprising the following steps: S1, polyvinyl chloride resin as the base material of the coil; S2, the conductive filler is selected as electric carbon black and metal powder, the metal powder is the following weight parts, 15-35 parts of aluminum powder, 10-25 parts of scandium powder, 15-25 parts of nickel powder, 10-30 parts of aluminum silicon magnesium powder, 10-30 parts of graphene powder are mixed to form the metal powder; S3, adding polyvinyl chloride resin, electric carbon black and metal powder in sequence and mixing them by a mixing device, wherein the mixing temperature in the mixing device is 160° C. to 180° C., the stirring time in the mixing device is 20 minutes to 40 minutes, and a stirring material is formed after the mixing is completed; S4. After forming the stirring material, a stabilizer is added into the mixing equipment. The stabilizer is one of tribasic lead sulfate, calcium stearate, barium stearate, and zinc stearate. After adding the stabilizer, the mixing temperature in the mixing equipment is 120° C. to 140° C., and the stirring time in the mixing equipment is 10 minutes to 20 minutes. After the mixing is completed, the raw material is formed; S5, putting the raw material into an extruder for extrusion of a coil, the extrusion pressure of the extruder is 0.022~0.45MPa, the extrusion speed is 2~3m / min, and the raw material after extrusion is coil A; S6. During the extrusion process of coil A, the surface of coil A is coated with a conductive coating, and the conductive coating forms a continuous conductive network to improve its electrostatic conductivity. The conductive network is in a grid shape. After the surface of coil A is coated with the conductive coating, coil C is formed. S7, the conductive coating is a mixture of the following materials in parts by weight: 20-30 parts of graphite, 10-15 parts of graphite fiber, 12-18 parts of carbon fiber, 8-15 parts of graphene, and 100-200 parts of water, and stirred at a temperature of 40°C-60°C for 10-20 minutes; S8. After coil C is formed, it is cooled quickly to ensure that coil C is cooled quickly after forming to reduce thermal deformation.

[0006] Preferably, the rapid cooling is performed by spraying water to quickly reduce the temperature, the temperature of the sprayed water is 0-5°C, and the coiled material is solidified during the spraying of water.

[0007] Preferably, the curing treatment is to spray water at a temperature of 0-5° C. for 5-10 minutes to cure the coiled material.

[0008] Preferably, after the coil is cured, the conductive property of the coil is monitored in real time by a conductive testing device, and the testing time of the conductive testing device is 5 minutes.

[0009] Preferably, the polyvinyl chloride resin is washed in water for 5 minutes to clean impurities, and the polyvinyl chloride resin with impurities cleaned is placed in a dryer for drying. The temperature in the dryer is 70-90° C. and the drying time of the dryer is 15-20 minutes to ensure the quality of the base material.

[0010] Preferably, the conductive coating is directly attached to the surface of the coil A using conductive polymer as a basic film-forming substance without the need for other adhesives.

[0011] Preferably, the conductive filler is pre-dispersed with the assistance of ultrasound, and the frequency of the ultrasound is 42KHz~58KHz.

[0012] Preferably, the base material is divided into blocks by strong shearing, and the divided blocks are put into a mixing device for mixing, which effectively improves the mixing efficiency.

[0013] Preferably, the particle size of the metal powder is 20-40 μm.

[0014] Preferably, it comprises a roll body, a filler layer and a conductive layer, the outer wall of the roll body is wrapped with the filler layer, the outer wall of the filler layer is installed with the conductive layer, the roll body is the base material, the filler layer is the conductive filler, and the conductive layer is the conductive coating.

[0015] Compared with the prior art, the present invention has the following beneficial effects: 1. The present invention is provided with a conductive filler selected as electric carbon black and metal powder, wherein the metal powder is the following weight parts, 28 parts of aluminum powder, 24 parts of scandium powder, 23 parts of nickel powder, 26 parts of aluminum silicon magnesium powder, and 24 parts of graphene powder. The polyvinyl chloride resin, the electric carbon black and the metal powder are added in sequence by a mixing device for mixing. The mixing temperature in the mixing device is 160° C. to 180° C., and the stirring time in the mixing device is 20 minutes to 40 minutes. After the mixing is completed, a stirring material is formed. After the stirring material is formed, a stabilizer is added to the mixing device. The stabilizer is one of tribasic lead sulfate, calcium stearate, barium stearate, and zinc stearate. After the stabilizer is added, the mixing temperature in the mixing device is 130° C., and the stirring time in the mixing device is 19 minutes. After the mixing is completed, The raw materials are formed, and the raw materials are put into an extruder for extrusion of coils. The extrusion pressure of the extruder is 0.022~0.45MPa, and the extrusion speed is 2~3m / min. The extruded raw material is coil A. During the extrusion of coil A, the surface of coil A is coated with conductive coating, and the conductive coating forms a continuous conductive network to improve its electrostatic conductivity. The conductive network is in a grid shape. The surface of coil A is coated with conductive coating to form coil C. The conductive coating is a mixture of the following materials by weight: 27 parts of graphite, 13 parts of graphite fiber, 16 parts of carbon fiber, 12 parts of graphene, and 160 parts of water. The materials are stirred at a temperature of 56°C for 12 minutes, thereby improving the conductivity of the PVC coil and greatly improving the electrostatic conductivity of the PVC coil, thereby improving safety. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 It is a front view structural schematic diagram of the present invention; Figure 2 It is a schematic diagram of the cross-sectional structure of the present invention.

[0017] In the figure: 1, coil body; 2, filler layer; 3, conductive layer. DETAILED DESCRIPTION

[0018] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0019] In the description of the present invention, it should be noted that the terms "upper", "lower", "inner", "outer", "front end", "rear end", "two ends", "one end", "the other end" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first" and "second" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance.

[0020] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "provided with", "connected", etc. should be understood in a broad sense. For example, "connected" can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0021] Embodiment 1: An embodiment provided by the present invention: A process for preparing a PVC coiled material with a static conductive function, comprising the following steps: S1, polyvinyl chloride resin as the base material of the coil; S2, the conductive filler is selected as electric carbon black and metal powder, the metal powder is the following parts by weight, 16 parts of aluminum powder, 12 parts of scandium powder, 17 parts of nickel powder, 12 parts of aluminum silicon magnesium powder, and 12 parts of graphene powder are mixed to form the metal powder; S3, adding polyvinyl chloride resin, electric carbon black and metal powder in sequence and mixing them by a mixing device, wherein the mixing temperature in the mixing device is 160° C. to 180° C., the stirring time in the mixing device is 20 minutes to 40 minutes, and a stirring material is formed after the mixing is completed; S4. After forming the stirring material, a stabilizer is added to the mixing device. The stabilizer is one of tribasic lead sulfate, calcium stearate, barium stearate, and zinc stearate. After adding the stabilizer, the mixing temperature in the mixing device is 122° C. The stirring time in the mixing device is 12 minutes. After the mixing is completed, the raw material is formed; S5, putting the raw material into an extruder for extrusion of a coil, the extrusion pressure of the extruder is 0.022~0.45MPa, the extrusion speed is 2~3m / min, and the raw material after extrusion is coil A; S6. During the extrusion process of coil A, the surface of coil A is coated with a conductive coating, and the conductive coating forms a continuous conductive network to improve its electrostatic conductivity. The conductive network is in a grid shape. After the surface of coil A is coated with the conductive coating, coil C is formed. S7, the conductive coating is mixed with the following materials in parts by weight: 22 parts of graphite, 11 parts of graphite fiber, 13 parts of carbon fiber, 10 parts of graphene, and 120 parts of water, and stirred at a temperature of 42° C. for 12 minutes; S8. After the coil C is formed, it is cooled quickly to ensure that the coil C is cooled quickly after forming to reduce thermal deformation. The rapid cooling is carried out by spraying water. The temperature of the water spray is 0~5℃. The coil is cured during the water spraying. The curing treatment is to spray the water at a temperature of 0~5℃ for 5~10 minutes to cure the coil. After the coil is cured, it is tested by the conductivity test equipment to monitor the conductivity of the coil in real time. The test time of the conductivity test equipment is 5 minutes. The polyvinyl chloride resin is washed in water for 5 minutes to clean the impurities. The polyvinyl chloride resin with clean impurities is put into the dryer for drying. The temperature in the dryer is 70~90℃. The drying time of the dryer is The mixing time is 15 to 20 minutes to ensure the quality of the basic material. The conductive coating is directly attached to the surface of coil A with conductive polymer as the basic film-forming material, without other adhesives. The conductive filler is pre-dispersed with the assistance of ultrasound, and the ultrasonic frequency is 42KHz to 58KHz. The basic material is divided into blocks by strong shearing, and the blocks are put into the mixing equipment for mixing, which effectively improves the mixing efficiency. The particle size of the metal powder is 20 to 40μm, including a coil body 1, a filler layer 2 and a conductive layer 3. The outer wall of the coil body 1 is wrapped with the filler layer 2, and the outer wall of the filler layer 2 is installed with the conductive layer 3. The coil body 1 is the basic material, the filler layer 2 is a conductive filler, and the conductive layer 3 is a conductive coating.

[0022] Embodiment 2: An embodiment provided by the present invention: A process for preparing a PVC coiled material with a static conductive function, comprising the following steps: S1, polyvinyl chloride resin as the base material of the coil; S2, the conductive filler is selected as electric carbon black and metal powder, the metal powder is the following parts by weight, 20 parts of aluminum powder, 15 parts of scandium powder, 18 parts of nickel powder, 15 parts of aluminum silicon magnesium powder, and 18 parts of graphene powder are mixed to form the metal powder; S3, adding polyvinyl chloride resin, electric carbon black and metal powder in sequence and mixing them by a mixing device, wherein the mixing temperature in the mixing device is 160° C. to 180° C., the stirring time in the mixing device is 20 minutes to 40 minutes, and a stirring material is formed after the mixing is completed; S4. After forming the stirring material, a stabilizer is added to the mixing device. The stabilizer is one of tribasic lead sulfate, calcium stearate, barium stearate, and zinc stearate. After adding the stabilizer, the mixing temperature in the mixing device is 125° C. The stirring time in the mixing device is 16 minutes. After the mixing is completed, the raw material is formed; S5, putting the raw material into an extruder for extrusion of a coil, the extrusion pressure of the extruder is 0.022~0.45MPa, the extrusion speed is 2~3m / min, and the raw material after extrusion is coil A; S6. During the extrusion process of coil A, the surface of coil A is coated with a conductive coating, and the conductive coating forms a continuous conductive network to improve its electrostatic conductivity. The conductive network is in a grid shape. After the surface of coil A is coated with the conductive coating, coil C is formed. S7, the conductive coating is mixed with the following materials in parts by weight: 26 parts of graphite, 12 parts of graphite fiber, 14 parts of carbon fiber, 11 parts of graphene, and 140 parts of water, and stirred at a temperature of 50° C. for 15 minutes; S8. After the coil C is formed, it is cooled quickly to ensure that the coil C is cooled quickly after forming to reduce thermal deformation. The rapid cooling is carried out by spraying water. The temperature of the water spray is 0~5℃. The coil is cured during the water spraying. The curing treatment is to spray the water at a temperature of 0~5℃ for 5~10 minutes to cure the coil. After the coil is cured, it is tested by the conductivity test equipment to monitor the conductivity of the coil in real time. The test time of the conductivity test equipment is 5 minutes. The polyvinyl chloride resin is washed in water for 5 minutes to clean the impurities. The polyvinyl chloride resin with clean impurities is put into the dryer for drying. The temperature in the dryer is 70~90℃. The drying time of the dryer is The mixing time is 15 to 20 minutes to ensure the quality of the basic material. The conductive coating is directly attached to the surface of coil A with conductive polymer as the basic film-forming material, without other adhesives. The conductive filler is pre-dispersed with the assistance of ultrasound, and the ultrasonic frequency is 42KHz to 58KHz. The basic material is divided into blocks by strong shearing, and the blocks are put into the mixing equipment for mixing, which effectively improves the mixing efficiency. The particle size of the metal powder is 20 to 40μm, including a coil body 1, a filler layer 2 and a conductive layer 3. The outer wall of the coil body 1 is wrapped with the filler layer 2, and the outer wall of the filler layer 2 is installed with the conductive layer 3. The coil body 1 is the basic material, the filler layer 2 is a conductive filler, and the conductive layer 3 is a conductive coating.

[0023] Embodiment 3: An embodiment provided by the present invention: A process for preparing a PVC coiled material with a static conductive function, comprising the following steps: S1, polyvinyl chloride resin as the base material of the coil; S2, the conductive filler is selected as electric carbon black and metal powder, the metal powder is the following parts by weight, 25 parts of aluminum powder, 20 parts of scandium powder, 18 parts of nickel powder, 20 parts of aluminum silicon magnesium powder, 23 parts of graphene powder are mixed to form the metal powder; S3, adding polyvinyl chloride resin, electric carbon black and metal powder in sequence and mixing them by a mixing device, wherein the mixing temperature in the mixing device is 160° C. to 180° C., the stirring time in the mixing device is 20 minutes to 40 minutes, and a stirring material is formed after the mixing is completed; S4. After forming the stirring material, a stabilizer is added to the mixing device. The stabilizer is one of tribasic lead sulfate, calcium stearate, barium stearate, and zinc stearate. After adding the stabilizer, the mixing temperature in the mixing device is 128° C. The stirring time in the mixing device is 18 minutes. After the mixing is completed, the raw material is formed; S5, putting the raw material into an extruder for extrusion of a coil, the extrusion pressure of the extruder is 0.022~0.45MPa, the extrusion speed is 2~3m / min, and the raw material after extrusion is coil A; S6. During the extrusion process of coil A, the surface of coil A is coated with a conductive coating, and the conductive coating forms a continuous conductive network to improve its electrostatic conductivity. The conductive network is in a grid shape. After the surface of coil A is coated with the conductive coating, coil C is formed. S7, the conductive coating is mixed with the following materials in parts by weight: 29 parts of graphite, 14 parts of graphite fiber, 17 parts of carbon fiber, 14 parts of graphene, and 160 parts of water, and stirred at a temperature of 55° C. for 18 minutes; S8. After the coil C is formed, it is cooled quickly to ensure that the coil C is cooled quickly after forming to reduce thermal deformation. The rapid cooling is carried out by spraying water. The temperature of the water spray is 0~5℃. The coil is cured during the water spraying. The curing treatment is to spray the water at a temperature of 0~5℃ for 5~10 minutes to cure the coil. After the coil is cured, it is tested by the conductivity test equipment to monitor the conductivity of the coil in real time. The test time of the conductivity test equipment is 5 minutes. The polyvinyl chloride resin is washed in water for 5 minutes to clean the impurities. The polyvinyl chloride resin with clean impurities is put into the dryer for drying. The temperature in the dryer is 70~90℃. The drying time of the dryer is The mixing time is 15 to 20 minutes to ensure the quality of the basic material. The conductive coating is directly attached to the surface of coil A with conductive polymer as the basic film-forming material, without other adhesives. The conductive filler is pre-dispersed with the assistance of ultrasound, and the ultrasonic frequency is 42KHz to 58KHz. The basic material is divided into blocks by strong shearing, and the blocks are put into the mixing equipment for mixing, which effectively improves the mixing efficiency. The particle size of the metal powder is 20 to 40μm, including a coil body 1, a filler layer 2 and a conductive layer 3. The outer wall of the coil body 1 is wrapped with the filler layer 2, and the outer wall of the filler layer 2 is installed with the conductive layer 3. The coil body 1 is the basic material, the filler layer 2 is a conductive filler, and the conductive layer 3 is a conductive coating.

[0024] Embodiment 4: An embodiment provided by the present invention: A process for preparing a PVC coiled material with a static conductive function, comprising the following steps: S1, polyvinyl chloride resin as the base material of the coil; S2, the conductive filler is selected as electric carbon black and metal powder, the metal powder is the following parts by weight, 28 parts of aluminum powder, 24 parts of scandium powder, 23 parts of nickel powder, 26 parts of aluminum silicon magnesium powder, and 24 parts of graphene powder are mixed to form the metal powder; S3, adding polyvinyl chloride resin, electric carbon black and metal powder in sequence and mixing them by a mixing device, wherein the mixing temperature in the mixing device is 160° C. to 180° C., the stirring time in the mixing device is 20 minutes to 40 minutes, and a stirring material is formed after the mixing is completed; S4. After forming the stirring material, a stabilizer is added to the mixing device. The stabilizer is one of tribasic lead sulfate, calcium stearate, barium stearate, and zinc stearate. After adding the stabilizer, the mixing temperature in the mixing device is 130° C. The stirring time in the mixing device is 19 minutes. After the mixing is completed, the raw material is formed; S5, putting the raw material into an extruder for extrusion of a coil, the extrusion pressure of the extruder is 0.022~0.45MPa, the extrusion speed is 2~3m / min, and the raw material after extrusion is coil A; S6. During the extrusion process of coil A, the surface of coil A is coated with a conductive coating, and the conductive coating forms a continuous conductive network to improve its electrostatic conductivity. The conductive network is in a grid shape. After the surface of coil A is coated with the conductive coating, coil C is formed. S7, the conductive coating is mixed with the following materials in parts by weight: 27 parts of graphite, 13 parts of graphite fiber, 16 parts of carbon fiber, 12 parts of graphene, and 160 parts of water, and stirred at a temperature of 56° C. for 12 minutes; S8. After the coil C is formed, it is cooled quickly to ensure that the coil C is cooled quickly after forming to reduce thermal deformation. The rapid cooling is carried out by spraying water. The temperature of the water spray is 0~5℃. The coil is cured during the water spraying. The curing treatment is to spray the water at a temperature of 0~5℃ for 5~10 minutes to cure the coil. After the coil is cured, it is tested by the conductivity test equipment to monitor the conductivity of the coil in real time. The test time of the conductivity test equipment is 5 minutes. The polyvinyl chloride resin is washed in water for 5 minutes to clean the impurities. The polyvinyl chloride resin with clean impurities is put into the dryer for drying. The temperature in the dryer is 70~90℃. The drying time of the dryer is The mixing time is 15 to 20 minutes to ensure the quality of the basic material. The conductive coating is directly attached to the surface of coil A with conductive polymer as the basic film-forming material, without other adhesives. The conductive filler is pre-dispersed with the assistance of ultrasound, and the ultrasonic frequency is 42KHz to 58KHz. The basic material is divided into blocks by strong shearing, and the blocks are put into the mixing equipment for mixing, which effectively improves the mixing efficiency. The particle size of the metal powder is 20 to 40μm, including a coil body 1, a filler layer 2 and a conductive layer 3. The outer wall of the coil body 1 is wrapped with the filler layer 2, and the outer wall of the filler layer 2 is installed with the conductive layer 3. The coil body 1 is the basic material, the filler layer 2 is a conductive filler, and the conductive layer 3 is a conductive coating.

[0025] Embodiment 5: An embodiment provided by the present invention: A process for preparing a PVC coiled material with a static conductive function, comprising the following steps: S1, polyvinyl chloride resin as the base material of the coil; S2, the conductive filler is selected as electric carbon black and metal powder, the metal powder is the following parts by weight, 33 parts of aluminum powder, 22 parts of scandium powder, 23 parts of nickel powder, 26 parts of aluminum silicon magnesium powder, and 19 parts of graphene powder are mixed to form the metal powder; S3, adding polyvinyl chloride resin, electric carbon black and metal powder in sequence and mixing them by a mixing device, wherein the mixing temperature in the mixing device is 160° C. to 180° C., the stirring time in the mixing device is 20 minutes to 40 minutes, and a stirring material is formed after the mixing is completed; S4. After forming the stirring material, a stabilizer is added to the mixing device. The stabilizer is one of tribasic lead sulfate, calcium stearate, barium stearate, and zinc stearate. After adding the stabilizer, the mixing temperature in the mixing device is 135° C. The stirring time in the mixing device is 15 minutes. After the mixing is completed, the raw material is formed; S5, putting the raw material into an extruder for extrusion of a coil, the extrusion pressure of the extruder is 0.022~0.45MPa, the extrusion speed is 2~3m / min, and the raw material after extrusion is coil A; S6. During the extrusion process of coil A, the surface of coil A is coated with a conductive coating, and the conductive coating forms a continuous conductive network to improve its electrostatic conductivity. The conductive network is in a grid shape. After the surface of coil A is coated with the conductive coating, coil C is formed. S7, the conductive coating is mixed with the following materials in parts by weight: 26 parts of graphite, 13 parts of graphite fiber, 15 parts of carbon fiber, 13 parts of graphene, and 180 parts of water, and stirred at a temperature of 53° C. for 16 minutes; S8. After the coil C is formed, it is cooled quickly to ensure that the coil C is cooled quickly after forming to reduce thermal deformation. The rapid cooling is carried out by spraying water. The temperature of the water spray is 0~5℃. The coil is cured during the water spraying. The curing treatment is to spray the water at a temperature of 0~5℃ for 5~10 minutes to cure the coil. After the coil is cured, it is tested by the conductivity test equipment to monitor the conductivity of the coil in real time. The test time of the conductivity test equipment is 5 minutes. The polyvinyl chloride resin is washed in water for 5 minutes to clean the impurities. The polyvinyl chloride resin with clean impurities is put into the dryer for drying. The temperature in the dryer is 70~90℃. The drying time of the dryer is The mixing time is 15 to 20 minutes to ensure the quality of the basic material. The conductive coating is directly attached to the surface of coil A with conductive polymer as the basic film-forming material, without other adhesives. The conductive filler is pre-dispersed with the assistance of ultrasound, and the ultrasonic frequency is 42KHz to 58KHz. The basic material is divided into blocks by strong shearing, and the blocks are put into the mixing equipment for mixing, which effectively improves the mixing efficiency. The particle size of the metal powder is 20 to 40μm, including a coil body 1, a filler layer 2 and a conductive layer 3. The outer wall of the coil body 1 is wrapped with the filler layer 2, and the outer wall of the filler layer 2 is installed with the conductive layer 3. The coil body 1 is the basic material, the filler layer 2 is a conductive filler, and the conductive layer 3 is a conductive coating.

[0026] Comparative experiment: The difference between Comparative Example 1 and Example 1 is that; The conductive filler is selected as electric carbon black and metal powder. The metal powder is the following parts by weight: 16 parts of aluminum powder, 12 parts of scandium powder, 17 parts of nickel powder, 12 parts of aluminum silicon magnesium powder, and 12 parts of graphene powder are mixed to form metal powder. After forming the stirring material, a stabilizer is added to the mixing equipment. The stabilizer is one of tribasic lead sulfate, calcium stearate, barium stearate, and zinc stearate. After adding the stabilizer, the mixing temperature in the mixing equipment is 122°C, and the stirring time in the mixing equipment is 12 minutes. After mixing, the raw material is formed. The conductive coating is a mixture of the following parts by weight: 22 parts of graphite, 11 parts of graphite fiber, 13 parts of carbon fiber, 10 parts of graphene, and 120 parts of water. It is stirred at a temperature of 42°C for 12 minutes.

[0027] The difference between Comparative Example 1 and Example 2 is that; The conductive filler is selected as electric carbon black and metal powder. The metal powder is the following parts by weight: 20 parts of aluminum powder, 15 parts of scandium powder, 18 parts of nickel powder, 15 parts of aluminum silicon magnesium powder, and 18 parts of graphene powder are mixed to form metal powder. After forming the stirring material, a stabilizer is added to the mixing equipment. The stabilizer is one of tribasic lead sulfate, calcium stearate, barium stearate, and zinc stearate. After adding the stabilizer, the mixing temperature in the mixing equipment is 125°C, and the stirring time in the mixing equipment is 16 minutes. After mixing, the raw material is formed. The conductive coating is a mixture of the following parts by weight: 26 parts of graphite, 12 parts of graphite fiber, 14 parts of carbon fiber, 11 parts of graphene, and 140 parts of water. It is stirred at a temperature of 50°C for 15 minutes.

[0028] The difference between Comparative Example 1 and Example 3 is that; The conductive filler is selected as electric carbon black and metal powder. The metal powder is the following parts by weight: 25 parts of aluminum powder, 20 parts of scandium powder, 18 parts of nickel powder, 20 parts of aluminum silicon magnesium powder, and 23 parts of graphene powder are mixed to form metal powder. After forming the stirring material, a stabilizer is added to the mixing equipment. The stabilizer is one of tribasic lead sulfate, calcium stearate, barium stearate, and zinc stearate. After adding the stabilizer, the mixing temperature in the mixing equipment is 128°C, and the stirring time in the mixing equipment is 18 minutes. After mixing, the raw material is formed. The conductive coating is a mixture of the following parts by weight: 29 parts of graphite, 14 parts of graphite fiber, 17 parts of carbon fiber, 14 parts of graphene, and 160 parts of water. It is stirred at a temperature of 55°C for 18 minutes.

[0029] The difference between Comparative Example 1 and Example 4 is that; The conductive filler is selected as electric carbon black and metal powder. The metal powder is the following parts by weight: 28 parts of aluminum powder, 24 parts of scandium powder, 23 parts of nickel powder, 26 parts of aluminum silicon magnesium powder, and 24 parts of graphene powder are mixed to form metal powder. After forming the stirring material, a stabilizer is added to the mixing equipment. The stabilizer is one of tribasic lead sulfate, calcium stearate, barium stearate, and zinc stearate. After adding the stabilizer, the mixing temperature in the mixing equipment is 130°C, and the stirring time in the mixing equipment is 19 minutes. After mixing, the raw material is formed. The conductive coating is a mixture of the following parts by weight: 27 parts of graphite, 13 parts of graphite fiber, 16 parts of carbon fiber, 12 parts of graphene, and 160 parts of water. It is stirred at a temperature of 56°C for 12 minutes.

[0030] The difference between Comparative Example 1 and Example 5 is that; The conductive filler is selected as electric carbon black and metal powder. The metal powder is the following parts by weight: 33 parts of aluminum powder, 22 parts of scandium powder, 23 parts of nickel powder, 26 parts of aluminum silicon magnesium powder, and 19 parts of graphene powder are mixed to form metal powder. After forming the stirring material, a stabilizer is added to the mixing equipment. The stabilizer is one of tribasic lead sulfate, calcium stearate, barium stearate, and zinc stearate. After adding the stabilizer, the mixing temperature in the mixing equipment is 135°C, and the stirring time in the mixing equipment is 15 minutes. After mixing, the raw material is formed. The conductive coating is a mixture of the following parts by weight: 26 parts of graphite, 13 parts of graphite fiber, 15 parts of carbon fiber, 13 parts of graphene, and 180 parts of water. It is stirred at a temperature of 53°C for 16 minutes.

[0031] The PVC coils with static electricity conduction function of Examples 1, 2, 3, 4 and 5 of the present invention and the conventional PVC coils with static electricity conduction function (Comparative Example 1) were respectively tested for conductivity and wear resistance, and their values ​​were calculated and statistically analyzed. The results are shown in Table 1.

[0032] Table 1 From the data in Table 1, it can be seen that the conductivity of the PVC coiled material with a static conductive function in Examples 1, 2, 3, 4 and 5 of the present invention is 0.01, 0.011, 0.013, 0.011 and 0.012, respectively, which are significantly higher than the conductivity of the traditional static conductive PVC coiled material in Comparative Example 1. Therefore, it is shown that the conductivity of the PVC coiled material with a static conductive function of the present invention is significantly improved, thereby improving the static conductive effect.

[0033] From the data in Table 1, it can be seen that the wear resistance of the PVC coil with static electricity conduction function in Examples 1, 2, 3, 4 and 5 of the present invention are 50, 48, 51, 49 and 52 respectively, which are significantly higher than the wear resistance of the traditional PVC coil with static electricity conduction function in Comparative Example 1. Therefore, it is shown that the wear resistance of the PVC coil with static electricity conduction function of the present invention is significantly improved, and the wear resistance effect of the PVC coil is improved.

[0034] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.

Claims

1. A process for preparing a PVC coiled material with a static conductive function, characterized in that: The following steps are involved: S1, polyvinyl chloride resin as the base material of the coil; S2, the conductive filler is selected as electric carbon black and metal powder, the metal powder is the following weight parts, 15-35 parts of aluminum powder, 10-25 parts of scandium powder, 15-25 parts of nickel powder, 10-30 parts of aluminum silicon magnesium powder, 10-30 parts of graphene powder are mixed to form the metal powder; S3, adding polyvinyl chloride resin, electric carbon black and metal powder in sequence and mixing them by a mixing device, wherein the mixing temperature in the mixing device is 160° C. to 180° C., the stirring time in the mixing device is 20 minutes to 40 minutes, and a stirring material is formed after the mixing is completed; S4. After forming the stirring material, a stabilizer is added into the mixing equipment. The stabilizer is one of tribasic lead sulfate, calcium stearate, barium stearate, and zinc stearate. After adding the stabilizer, the mixing temperature in the mixing equipment is 120° C. to 140° C., and the stirring time in the mixing equipment is 10 minutes to 20 minutes. After the mixing is completed, the raw material is formed; S5, putting the raw material into an extruder for extrusion of a coil, the extrusion pressure of the extruder is 0.022~0.45MPa, the extrusion speed is 2~3m / min, and the raw material after extrusion is coil A; S6. During the extrusion process of coil A, the surface of coil A is coated with a conductive coating, and the conductive coating forms a continuous conductive network to improve its electrostatic conductivity. The conductive network is in a grid shape. After the surface of coil A is coated with the conductive coating, coil C is formed. S7, the conductive coating is a mixture of the following materials in parts by weight: 20-30 parts of graphite, 10-15 parts of graphite fiber, 12-18 parts of carbon fiber, 8-15 parts of graphene, and 100-200 parts of water, and stirred at a temperature of 40°C-60°C for 10-20 minutes; S8. After the coil C is formed, it is cooled quickly to ensure that the coil C is cooled quickly after forming to reduce thermal deformation.

2. The process for preparing a PVC coiled material with a static conductive function according to claim 1, characterized in that: The rapid cooling is carried out by spraying water to quickly reduce the temperature, the temperature of the sprayed water is 0-5°C, and the coiled material is solidified during the spraying of water.

3. The process for preparing a PVC coiled material with a static conductive function according to claim 2, characterized in that: The curing treatment is to spray water at a temperature of 0 to 5° C. for 5 to 10 minutes to cure the coiled material.

4. The process for preparing a PVC coiled material with a static conductive function according to claim 3, characterized in that: After the coil is cured, the conductive property of the coil is monitored in real time by a conductive testing device, and the testing time of the conductive testing device is 5 minutes.

5. The process for preparing a PVC coiled material with a static conductive function according to claim 1, characterized in that: The polyvinyl chloride resin is washed in water for 5 minutes to clean impurities, and the polyvinyl chloride resin with impurities cleaned is put into a dryer for drying. The temperature in the dryer is 70-90° C. and the drying time of the dryer is 15-20 minutes to ensure the quality of the basic material.

6. The process for preparing a PVC coiled material with a static conductive function according to claim 1, characterized in that: The conductive coating is directly attached to the surface of the coil A using conductive polymer as a basic film-forming substance without the need for other adhesives.

7. The process for preparing a PVC coiled material with a static conductive function according to claim 1, characterized in that: The conductive filler is pre-dispersed with the assistance of ultrasound, and the ultrasound frequency is 42KHz~58KHz.

8. The process for preparing a PVC coiled material with a static conductive function according to claim 1, characterized in that: The base material is divided into blocks by strong shearing, and the divided blocks are put into a mixing device for mixing, thereby effectively improving the mixing efficiency.

9. The process for preparing a PVC coiled material with a static conductive function according to claim 1, characterized in that: The particle size of the metal powder is 20-40 μm.

10. The PVC coiled material prepared by the process for preparing a PVC coiled material with static conductive function according to any one of claims 1 to 9, characterized in that: The invention comprises a roll body (1), a filler layer (2) and a conductive layer (3); the outer wall of the roll body (1) is wrapped with the filler layer (2); the outer wall of the filler layer (2) is installed with the conductive layer (3); the roll body (1) is the base material, the filler layer (2) is the conductive filler, and the conductive layer (3) is the conductive coating.