Polypropylene foamed bead forming body as well as preparation method and application thereof

By adopting a multi-layer hot-pressed polypropylene composite sheet with high strength and high impact resistance, the physical properties and recycling and treatment of polypropylene foam bead molded body is solved, and efficient heat insulation and compression performance is improved, and simplified The recycling process is completed.

CN118909295APending Publication Date: 2024-11-08CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310513096.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-08
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

While improving physical properties, existing polypropylene foam bead molded bodies are difficult to reduce the apparent density and molding time, and are difficult to recover and process. Compared with other reinforcement materials, they have poor compatibility, which affects thermal insulation performance and production efficiency. .

Method used

Using high-strength, high-impact, multi-layer hot-pressed polypropylene composite sheet as preset material, the compression strength and thermal insulation properties of polypropylene foam beads are improved through specific laminated structures and composition designs, and during recycling No separation treatment is required, it is directly crushed, melted and repelled.

Benefits of technology

It significantly improves the compression strength and thermal insulation properties of the polypropylene foam bead molded body, reduces the apparent density and molding time, simplifies recycling and improves compatibility with other reinforcement materials, and is suitable for high-end applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention belongs to the technical field of high polymer materials, and particularly relates to a polypropylene foamed bead forming body as well as a preparation method and application thereof. The polypropylene foamed bead forming body comprises a plurality of reinforced preset materials and a polypropylene foamed bead material which is bonded with the reinforced preset materials through molding, and the reinforced preset materials comprise a polypropylene composite material; the polypropylene composite material comprises a plurality of polypropylene sheet layer unit groups which are sequentially stacked and comprise at least one same or different polypropylene sheet layer unit, and the structure of each polypropylene sheet layer unit is BiAiB'i; the melting point of the polypropylene composition Ai is larger than the melting points of Bi and B'i, and the average value of the melting points of all the outer layers in the ith group is larger than or equal to the average value of the melting points of all the outer layers in the (i-1) th group. The polypropylene foamed bead forming body has excellent compression strength, apparent density and forming performance, the compatibility is greatly improved, and separation treatment is not needed during recycling.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer materials, and in particular relates to a polypropylene foamed bead molding and a preparation method and application thereof. Background Art

[0002] Compared with traditional polystyrene (PS), polyethylene (PE), and polyurethane (PU) foam materials, polypropylene (PP) foam materials have the lowest bulk density, and the lightweight effect through foaming is more significant. The material has high strength, high heat resistance, and high toughness, and its application performance is perfect. It is well known that in addition to the common advantages of polypropylene foam materials, the most significant advantage of polypropylene foam beads and molded bodies is free formability. Polypropylene foam beads can be molded to obtain foam products with complex geometric shapes and high three-dimensional dimensional accuracy, which are widely used in new energy vehicles, 5G communications, drones, logistics, insulation, precision machinery and electronic turnover packaging.

[0003] As the demand for polypropylene foam beads in my country's automotive, packaging, food and other fields continues to increase, the domestic consumption of polypropylene foam beads in 2021 will be about 60,000 tons / year, with an annual growth rate of more than 15%. While the market is booming, the polypropylene foam beads industry chain is also increasingly hoping to promote polypropylene foam beads materials to more high-end applications, which requires further improving the physical properties of polypropylene foam beads molded products without increasing the production cost during molding.

[0004] Traditional methods such as optimizing raw materials and processes are no longer able to meet the needs of the market. The use of filler modification can effectively improve the physical properties of polypropylene foam beads, but it will also significantly weaken the foaming molding ability of special materials and the weight reduction effect of the product's appearance quality, and will increase the pressure holding time and steam consumption during the molding of polypropylene foam beads; by designing and adjusting the type and content of catalysts and comonomers to optimize the molecular structure of special materials for polypropylene foam beads, the physical properties of polypropylene foam beads products can be improved while also improving the foaming molding ability, but the production promotion cycle is long and the cost is high; optimizing the foaming molding process conditions of polypropylene foam beads requires upstream and downstream enterprises of polypropylene foam beads products to adjust the production process parameters and even equipment, which is difficult to be accepted by manufacturers.

[0005] In order to further improve the physical properties of polypropylene foam beads, inorganic or organic reinforcing sheets are first placed in the polypropylene foam beads forming mold, and then polypropylene foam beads are injected into the mold to form, which has become a new process scheme. The reinforcing sheets pre-placed in the existing technology have high requirements for mechanical properties, and mainly use composite materials such as aluminum alloy, stainless steel or glass fiber / carbon fiber reinforced nylon. After adding these reinforcing sheets, it is easy to produce compatibility problems with the polypropylene foam beads formed body, which not only makes it difficult to achieve ideal physical properties such as compression and heat insulation, but also even fails to form. Even if the polypropylene foam beads formed products that meet the product performance are successfully obtained, the presence of the reinforcing sheet brings problems such as high apparent density, long molding time and high energy consumption, and it is difficult to recycle after mixing materials other than polypropylene. If there is a high-strength and high-impact polypropylene composite sheet used as a pre-set sheet, the polypropylene composition identical to the pre-set sheet can be used as the matrix resin of the polypropylene foam beads. The polypropylene foam beads product does not need to be separated and processed during recycling, and can be directly crushed and melted, and granulated again. However, it is difficult for conventional polypropylene sheets to have both high strength and high impact resistance, and multi-layer hot-pressed self-reinforced polypropylene composite sheets often have low impact strength and interlayer peeling strength, and it is impossible to obtain a hot-pressed composite material with both good mechanical properties and high interlayer peeling strength. When the above-mentioned polypropylene sheets are used as reinforcing pre-setting materials in polypropylene foam beads, the compression strength of the polypropylene foam beads often cannot meet the application requirements of the downstream market.

[0006] Therefore, how to provide a polypropylene foam bead molding that can reduce the apparent density of the foam molding and have a high compression strength, while not significantly reducing the thermal insulation capacity and being easy to recycle, is a technical problem that needs to be solved at present. Summary of the invention

[0007] In view of the deficiencies of the above-mentioned prior art, the present invention provides a polypropylene foam bead molded body. The polypropylene foam bead molded body uses a high-strength and high-impact polypropylene composite sheet as a pre-set sheet. The polypropylene foam bead molded body has excellent compression strength, apparent density, molding performance, physical properties and thermal insulation performance. Compared with other non-polypropylene reinforced pre-set materials on the market, the compatibility is greatly improved, and no separation treatment is required during recycling. It can be directly crushed and melted, and then granulated and used again. It has broad market prospects in the field of polypropylene foam bead technology.

[0008] The first aspect of the present invention is to provide a polypropylene foamed bead molded body, comprising a plurality of reinforced pre-set materials and a polypropylene foamed bead material bonded to the reinforced pre-set materials by molding, wherein the reinforced pre-set materials comprise a polypropylene composite material;

[0009] The polypropylene composite material comprises a plurality of polypropylene sheet unit groups stacked in sequence; each polypropylene sheet unit group comprises at least one identical or different polypropylene sheet unit, and each polypropylene sheet unit comprises a core layer A i and located in the core layer A i The outer layer B on both sides i , B' i , structure B i A i B' i The structure of the polypropylene composite material is, from bottom to top, the nth group... the ith group... the second group, the first group, the second group... the ith group... the nth group, and the total number of stacked groups of polypropylene sheet unit groups is 2n-1; i and n are both integers not less than 2, and i≤n;

[0010] Among them, the core layer A in the polypropylene sheet unit i Containing polypropylene composition A i , outer layer B i With outer layer B' i The same or different, each corresponding to a polypropylene composition B i , polypropylene composition B' i ,

[0011] The polypropylene composition A i The melting point is greater than that of the polypropylene composition B i , the polypropylene composition B' i The average melting point of all outer layers in the i-th group is greater than or equal to the average melting point of all outer layers in the i-1-th group.

[0012] According to the present invention, the reinforced pre-set material comprises a polypropylene composite material. Preferably, the reinforced pre-set material is selected from a polypropylene composite material.

[0013] According to the present invention, in the structure of the polypropylene composite material, the upper i-th group and the lower i-th group may be the same or different.

[0014] In a preferred embodiment of the present invention, the polypropylene composition A i Melting point and polypropylene composition B i The difference in melting points, polypropylene composition A i The melting point of polypropylene composition B' i The difference in melting points is respectively greater than or equal to 5°C, preferably greater than or equal to 10°C, more preferably greater than or equal to 20°C; more preferably 20-60°C.

[0015] According to the present invention, the core layers in each polypropylene sheet unit can be made of the same material or different materials. There is no particular limitation on this. As long as A iThe melting point is greater than that of the polypropylene composition B i , polypropylene composition B' i The melting point can achieve better technical effects.

[0016] In a preferred embodiment of the present invention, the difference between the average melting point of all outer layers in the i-th group and the average melting point of all outer layers in the i-1-th group is the same or different, and is each 1-40°C, preferably 1-10°C, and more preferably 1-5°C.

[0017] According to the present invention, the total number of stacked groups of the polypropylene sheet unit group is 2n-1. The present invention has a wide selection range for the total number of stacked groups of the polypropylene sheet unit group. In a preferred embodiment of the present invention, 2≤n≤100 is selected, more preferably, 2≤n≤50, and further preferably, 2≤n≤30.

[0018] According to the present invention, the selection range of the number of polypropylene sheet units included in each polypropylene sheet unit group is relatively wide. In a preferred embodiment of the present invention, each polypropylene sheet unit group independently includes 1 to 10, preferably 1 to 5, more preferably 1 to 3 identical or different polypropylene sheet units, more preferably 1 polypropylene sheet unit. Preferably, the number of polypropylene sheet units included in each polypropylene sheet unit group is the same.

[0019] Preferably, but not necessarily, the melting point of any outer layer in each group is within ±10°C, within ±5°C, preferably within ±3°C, more preferably within ±1°C of the average melting point of all outer layers in the group.

[0020] In the embodiment where each polypropylene sheet unit group includes only one polypropylene sheet unit, for example, the structure of the polypropylene composite material can be B from bottom to top. n A n B' n ……B i A i B' i ...B2A2B'2, B1A1B'1, B2A2B'2...B i A i B' i ……B n A n B' n , the total number of stacked layers of the polypropylene sheet unit is 2n-1; i and n are both integers not less than 2, and i≤n.

[0021] In the embodiment where each polypropylene ply unit group includes 2 or more polypropylene ply units, for example, the structure of the i-th polypropylene ply unit group is B i1 A i1 B'i1 , B i2 A i2 B' i2 ……B ip A ip B' ip The structure of the polypropylene composite material can be sequentially as follows from bottom to top: n1 A n1 B' n1 , B n2 A n2 B' n2 ……B nq A nq B' nq )……(B i1 A i1 B' i1 , B i2 A i2 B' i2 ……B ip A ip B' ip )……(B 21 A 21 B' 21 , B 22 A 22 B' 22 ……B 2k A 2k B' 2k )(B 11 A 11 B' 11 , B 12 A 12 B' 12 ……B 1j A 1j B' 1j )(B 21 A 21 B' 21 , B 22 A 22 B' 22 ……B 2k A 2k B' 2k )……(B i1 A i1 B' i1 , B i2 A i2 B' i2 ……B ip A ip B' ip )……(B n1 A n1 B' n1 , B n2 An2 B' n2 ……B nq A nq B' nq ), the total number of stacked polypropylene sheet units is j+2k+...2p+...2q; j, k, p, q are each independently an integer not less than 2, preferably an integer from 2 to 10, more preferably from 2 to 5, and more preferably from 2 to 3.

[0022] According to the present invention, the core layer A in each polypropylene sheet unit i The thickness ratio of each polypropylene sheet unit has a wide selection range. In a preferred embodiment of the present invention, based on the total thickness of each polypropylene sheet unit, the core layer A in each polypropylene sheet unit is i The thickness of the core layer A accounts for 51%-89% of the total thickness, preferably 71%-89%, and more preferably 71%-80%. i The outer layer B on both sides i and B' i The thicknesses may be the same or different, preferably the same.

[0023] The thickness of each polypropylene sheet unit can be selected in a wide range. In a preferred embodiment of the present invention, the thickness of each polypropylene sheet unit is 10-1000 μm, preferably 30-500 μm, and more preferably 50-300 μm.

[0024] According to the present invention, the core layer A i , Outer layer B i , Outer layer B i The thickness can be controlled by the extruder melt pump during processing.

[0025] According to the present invention, the polypropylene composition A i Including but not limited to one or more of homopolymer polypropylene, random copolymer polypropylene, and impact copolymer polypropylene; polypropylene composition B i , B' i Each includes but is not limited to one or more of homopolymer polypropylene, random copolymer polypropylene, impact copolymer polypropylene, and optional thermal bonding enhancer y i .

[0026] According to the present invention, the polypropylene composition A i The material selection range is relatively wide. In a preferred embodiment of the present invention, the polypropylene composition A i It includes one or more of homopolymer polypropylene, random copolymer polypropylene and impact copolymer polypropylene.

[0027] In a more preferred embodiment of the present invention, the polypropylene composition A i Including homopolymer polypropylene iand impact copolymer polypropylene b i In a further more preferred embodiment of the present invention, the polypropylene composition A i Based on the total weight of i Comprising 50-99wt% homopolymer polypropylene a i , 1-50wt% impact copolymer polypropylene b i ; Further preferably, the polypropylene composition A i Including 70-90wt% homopolymer polypropylene a i , 10-30wt% impact copolymer polypropylene b i .

[0028] According to the present invention, the polypropylene composition B i , B' i Each comprises one or more of homopolymer polypropylene, random copolymer polypropylene and impact copolymer polypropylene; preferably the polypropylene composition B i and / or polypropylene composition B' i Also contains thermal bonding enhancer i .

[0029] In a more preferred embodiment of the present invention, the polypropylene composition B i , the polypropylene composition B' i Each comprising random copolymer polypropylene x i and thermal bonding enhancers i Preferably, the polypropylene composition B i , the polypropylene composition B' i Based on the total weight of each, the polypropylene composition B i , the polypropylene composition B' i Each comprising 70-99 wt% of random copolymer polypropylene x i , 1-30wt% thermal bonding enhancer i ; Further preferably, the polypropylene composition B i , the polypropylene composition B' i Each comprising 80-90 wt% of random copolymer polypropylene x i , 10-20wt% thermal bonding enhancer i .

[0030] According to the present invention, the homopolymer polypropylene a i The selection range is relatively wide. In a preferred embodiment of the present invention, the homopolymer polypropylene a iThe melting point is 150-170°C, preferably 160-170°C, and / or the isotacticity (mm) is not less than 96%, preferably not less than 97%, more preferably not less than 98%.

[0031] According to the present invention, the homopolymer polypropylene a i The melt flow rate selection range is relatively wide. Preferably, the homopolymer polypropylene a i The melt flow rate at 230° C. and a load of 2.16 kg is 0.5-50 g / 10 min, preferably 1-20 g / 10 min, and more preferably 2.5-18 g / 10 min.

[0032] According to the present invention, "and / or" means that it can be a situation where any one of the conditions exists alone, or it can be a situation where both conditions exist.

[0033] According to the present invention, the impact copolymer polypropylene b i The selection range is relatively wide. In a preferred embodiment of the present invention, the impact copolymer polypropylene b i The melting point is 150-170°C, the monomers of the impact-resistant copolymer polypropylene and propylene copolymer are ethylene or butene, preferably butene, and / or the cantilever beam impact strength of the impact-resistant copolymer polypropylene is not less than 20KJ / m 2 (23℃).

[0034] According to the present invention, the impact copolymer polypropylene b i The melt flow rate selection range is relatively wide. Preferably, the impact copolymer polypropylene b i The melt flow rate at 230° C. and a load of 2.16 kg is 0.5-50 g / 10 min, preferably 1-20 g / 10 min, and more preferably 2.5-18 g / 10 min.

[0035] According to the research conducted by the inventors, when the polypropylene composition A i When the melt mass flow rate and polymer composition ratio of the raw materials used are within the preferred range, the impact copolymer polypropylene b in the composition i It can absorb impact energy well, meet the requirements of impact performance, and make the sheet have good impact performance. i The medium and large molecular segments are relatively regular and crystallization occurs during the sheet preparation process, so the sheet also has good tensile properties.

[0036] In a preferred embodiment of the present invention, the core layer A i It also contains a β-crystal nucleating agent; preferably, the β-crystal nucleating agent is selected from at least one of condensed ring aromatic hydrocarbons, Group IIA two-component complexes, aromatic diamides, rare earth compounds and cyclic dicarboxylates.

[0037] According to the present invention, the amount of the β-crystal nucleating agent can be selected in a wide range. Preferably, the polypropylene composition A i The total amount is 100 parts by weight, the core layer A i The content of the β-crystal nucleating agent is 0.01-0.5 parts by weight. For example, the content of the β-crystal nucleating agent can be 0.01, 0.05, 0.1, 0.2, 0.3, 0.4, or 0.5 parts by weight.

[0038] In a preferred embodiment of the present invention, the random copolymer polypropylene x i The melting point is 110-150°C, preferably 120-140°C, preferably, the average melting point of all random copolymer polypropylenes in group i is greater than the average melting point of all random copolymer polypropylenes in group i-1, preferably the difference in melting point is 1-40°C, more preferably 1-10°C, most preferably 1-5°C; preferably, the random copolymer polypropylene x i It is a copolymer of propylene and ethylene and / or butene, preferably an ethylene-propylene-butene terpolymer and / or a propylene-ethylene binary copolymer.

[0039] According to the present invention, the random copolymer polypropylene x i The melt flow rate of the random copolymer polypropylene x is selected in a wide range. Preferably, the melt flow rate at 230°C and 2.16 kg load is 0.5-50 g / 10 min, preferably 1-20 g / 10 min, and more preferably 3-18 g / 10 min. i The molecular weight distribution Mw / Mn is 5-12, preferably 7-10.

[0040] In a preferred embodiment of the present invention, the heat-absorbing adhesive enhancer y i The melting point or viscosity flow temperature is 70-110°C. And / or, the thermal bonding enhancer y i One or more selected from polyolefin elastomer, EPDM rubber, SEBS, SBS, EVA, petroleum resin; preferably, the thermal adhesion enhancer y i It is a polyolefin elastomer and / or a petroleum resin.

[0041] In a preferred embodiment of the present invention, the polyolefin elastomer is preferably a copolymer elastomer of ethylene and propylene and / or α-olefin, the α-olefin is preferably a C4-C12 α-olefin, more preferably 1-butene and / or 1-octene; and / or the petroleum resin is a C5 and / or C9 hydrogenated petroleum resin with a softening point of 100-150°C; preferably a cyclopentadiene type resin.

[0042] According to the present invention, the thermal bonding enhancer yi The melt flow rate selection range is relatively wide. Preferably, the thermal bonding enhancer y i The melt flow rate at 190° C. and a load of 2.16 kg is 0.5-50 g / 10 min, preferably 1-20 g / 10 min, preferably 1-18 g / 10 min, and more preferably 3-18 g / 10 min.

[0043] According to the research conducted by the inventors, when the polypropylene composition B i And polypropylene composition B' i When the respective polymer composition ratios are within the above preferred ranges, the low melting point random copolymer polypropylene x i and thermal bonding enhancers i It can significantly reduce the hot pressing temperature and widen the hot pressing temperature window, and the thermal bonding enhancer i The sheet material is provided with good bonding performance, and the interlayer peeling strength is further improved. The polypropylene composite material as a prefabricated reinforced sheet material enables the polypropylene foamed bead molded body of the present invention to have higher compression strength.

[0044] According to the research conducted by the inventors, when the polypropylene composition A i Combination B with polypropylene i And polypropylene composition B' i The respective polymer composition ratios and polymer composition A i When the thickness distribution is within the above preferred range, the sheet preparation process can be further stabilized, so that the sheet has further better uniformity, tensile strength, impact resistance and interlayer peeling strength. The polypropylene composite material in this more preferred embodiment as a prefabricated reinforced sheet enables the polypropylene foam beads molded body of the present invention to have further higher compressive strength.

[0045] According to the present invention, the polypropylene sheet can be a film or can have a certain thickness. In the present invention, the polypropylene film is a form of the polypropylene sheet.

[0046] According to the present invention, the polypropylene sheet unit is a polypropylene sheet and / or a polypropylene fabric; the polypropylene sheet unit can be a polypropylene sheet or a polypropylene fabric. In a preferred embodiment of the present invention, the polypropylene sheet unit is a polypropylene sheet or a polypropylene fabric.

[0047] In a preferred embodiment of the present invention, the polypropylene sheet comprises a polypropylene composition A i , polypropylene composition B i , polypropylene composition B' i The components including are co-extruded to obtain the same.

[0048] In a preferred embodiment of the present invention, the polypropylene fabric is prepared by the following method: firstly i , polypropylene composition B i , polypropylene composition B' i The components including the polypropylene sheet are co-extruded to obtain the polypropylene sheet, and then the polypropylene sheet is woven to obtain the polypropylene fabric; preferably, the polypropylene fabric has a three-dimensional structure of plain, twill and / or satin.

[0049] According to the present invention, preferably, the polypropylene sheet units are connected by heat-compression bonding.

[0050] As an example, the polypropylene composite material is prepared by thermally pressing multiple layers of the polypropylene sheets and / or the polypropylene fabrics described above.

[0051] Preferably, the polypropylene fabric is stacked at 0-90° between the warp and the warp from top to bottom, preferably with 2 or more layers, more preferably 2-200 layers; most preferably 4-100 layers. The multi-layer polypropylene sheet is stacked at 0-90° along the machine direction from top to bottom, preferably with 2 or more layers, more preferably 2-200 layers; most preferably 4-100 layers. The surface density of the polypropylene composite material is greater than or equal to 110 g / m 2 , more preferably 110g / m 2 -14000g / m 2 ; Most preferably 220g / m 2 -7000g / m 2 In a preferred embodiment of the present invention, the polypropylene composition A contained in each layer of the stacked polypropylene fabric is i Can be the same or different, each layer contains polypropylene fabric A i can be independently selected from, preferably the polypropylene composition A of each layer i are the same.

[0052] In a preferred embodiment of the present invention, the polypropylene composite material has at least one of the following characteristics:

[0053] The longitudinal tensile strength is ≥150MPa, preferably ≥170MPa; more preferably ≥160MPa, and even more preferably ≥180MPa; the interlayer peel strength is ≥1N / mm, preferably ≥1.2N / mm; more preferably ≥1.3N / mm, and even more preferably ≥1.5N / mm.

[0054] The longitudinal tensile strength is measured according to the method specified in GB / T1040.1-2018, and the interlayer peel strength is measured according to the method specified in GB / T2358-98. The corresponding specimens in the above two tests are the standard specimens required in the above-mentioned test standards.

[0055] When the polypropylene composite material is obtained by hot pressing 5 polypropylene sheet units and the thickness of the polypropylene composite material is about 390 μm, the drop weight impact strength is ≥42 J, preferably ≥45 J.

[0056] The drop weight impact strength is measured according to the method specified in GB / T14153-1993, and the thickness of the sample is the thickness of the prepared product.

[0057] According to the present invention, the polypropylene composite material described above can be prepared by the following method, comprising stacking 2n-1 polypropylene sheet unit groups in the order of nth group...ith group...2nd group, 1st group, 2nd group...ith group...nth group, and then performing a step of hot pressing and fusing.

[0058] In the embodiment where each polypropylene sheet unit group includes only one polypropylene sheet unit, the preparation method comprises: i A i B' i The polypropylene sheet unit is as follows: n A n B' n ……B i A i B' i ...B2A2B'2, B1A1B'1, B2A2B'2...B i A i B' i ……B n A n B' n The layers are stacked in sequence, followed by a heat-pressing fusion step.

[0059] In an embodiment in which each polypropylene sheet unit group includes 2 or more polypropylene sheet units, the preparation method includes stacking the polypropylene sheet units of each polypropylene sheet unit group in sequence, and then stacking 2n-1 of the polypropylene sheet unit groups in sequence in the order of the nth group...the ith group...the second group, the first group, the second group...the ith group...the nth group, and then performing a step of hot pressing and fusing.

[0060] In a preferred embodiment of the present invention, the polypropylene composition A iThe preparation comprises melt blending the raw materials, such as at least one of the homopolymer polypropylene, random copolymer polypropylene and impact copolymer polypropylene. The polypropylene composition A i The conditions and equipment for melt blending are the same as those for melt blending of polyolefins in the prior art. Preferably, the melt temperature is 190-240° C., and the equipment is preferably a twin-screw extruder.

[0061] In a preferred embodiment of the present invention, the polypropylene composition B i , B' i The preparation comprises melt blending the raw materials, such as at least one of the homopolymer polypropylene, random copolymer polypropylene and impact copolymer polypropylene; the polypropylene composition B i , B' i The conditions and equipment for melt blending are the same as those for melt blending of polyolefins in the prior art. Preferably, the melt temperature is 190-240° C., and the equipment is preferably a twin-screw extruder.

[0062] In a preferred embodiment of the present invention, the temperatures of co-extrusion molding and casting are independently selected from 200-240°C; and / or the temperature of the calendering roll is 50-70°C.

[0063] In a preferred embodiment of the present invention, the stretching conditions include: the stretching temperature is 90-165°C, preferably 90-140°C, and more preferably 90-119°C; and / or the stretching ratio is 1-15 times, preferably 2-9 times.

[0064] In a preferred embodiment of the present invention, the width of the polypropylene sheet is 2-5 mm.

[0065] In a preferred embodiment of the present invention, the hot pressing conditions include: hot pressing temperature of 115-170°C, preferably 115-159°C, and more preferably 140-159°C; hot pressing pressure of 2-10MPa, preheating time of 5-600s, hot pressing time of 1-600s, and preferably 10-500s.

[0066] In a preferred embodiment of the present invention, the cooling and shaping pressure is 2-8 MPa, and the cooling time is 30s-700s.

[0067] In a preferred embodiment of the present invention, adjacent polypropylene fabrics of the laminate are placed at 0-90° between the warp directions; and / or adjacent polypropylene sheets of the laminate are placed at 0-90° along their respective machine directions, and the machine direction is the stretching direction (MD).

[0068] According to the present invention, the polypropylene foamed beads material contains the polypropylene composition A i At least one of and / or the polypropylene composition B i , polypropylene composition B' i At least one of the following, and optional auxiliary agents. In the composition, the polypropylene composition Ai and the polypropylene composition B i , polypropylene composition B' i At least one of the above can be mixed in any ratio between 0 and 100. The polypropylene foam beads are prepared from the raw materials of the above polypropylene foam beads.

[0069] Preferably, the auxiliary agent is selected from one or more of antioxidants, antistatic agents, lubricants, anti-aging agents, flame retardants, and color powders.

[0070] The composition may also contain one or more of the following processing aids commonly used in polypropylene foaming processes, such as but not limited to:

[0071] Graphite toner: added amount 1%-8%, preferably 2-5%; antioxidant: added amount 0.1-15‰, preferably 0.1-5‰; antistatic agent: added amount 0.1-10%, preferably 0.5-5%; lubricant: added amount 0.1-10%, preferably 0.5-3%; anti-aging agent: added amount 0.01-5%, preferably 0.1-2%. Flame retardant: added amount 0.1-25%, preferably 1-20%. The content of processing aids is well known in the industry and will not be repeated here.

[0072] The preparation method of the polypropylene composition provided by the present invention includes but is not limited to: after each component is measured according to the formula, it is added into a high-speed mixer, and continuously stirred at high speed for 1-10 minutes, preferably 2-5 minutes at room temperature, and then added into a twin-screw extruder, extruded at 180-230°C, and granulated.

[0073] As a preferred embodiment of the polypropylene foam beads, the preparation method of the foam beads comprises: adding a foaming agent to the polypropylene composition, and foaming the composition to form the foam beads.

[0074] Preferably, the polypropylene foam bead material contains a foaming agent and / or is foamed from an inorganic physical foaming agent; preferably, the inorganic physical foaming agent is selected from at least one of air, nitrogen, carbon dioxide, oxygen and water; and / or, the foaming agent is selected from a chemical foaming agent and / or an organic physical foaming agent; more preferably, the chemical foaming agent is selected from at least one of azodicarbonamide, p-toluenesulfonylhydrazide, semicarbazides, tetrazoles, sodium bicarbonate and sodium citrate; the organic physical foaming agent is selected from at least one of an aliphatic hydrocarbon foaming agent, an alicyclic hydrocarbon foaming agent, and a halogenated hydrocarbon foaming agent.

[0075] Further specifically, as an example, the foaming agent used in the present invention can be a chemical foaming agent or a physical foaming agent. Among them, the chemical foaming agent includes but is not limited to at least one of azodicarbonamide (AC foaming agent), p-toluenesulfonyl hydrazide, semicarbazide, tetrazole, sodium bicarbonate and sodium citrate. The physical foaming agent can be an organic physical foaming agent or an inorganic physical foaming agent. Organic physical foaming agents include but are not limited to aliphatic hydrocarbons such as propane, butane, pentane, hexane and heptane, alicyclic hydrocarbons such as cyclobutane and cyclohexane, and halogenated hydrocarbons such as chlorofluoromethane, trifluoromethane, 1,2-difluoroethane, 1,2,2,2-tetrafluoroethane, methyl chloride, ethyl chloride and dichloromethane. The inorganic physical foaming agent includes but is not limited to at least one of air, nitrogen, carbon dioxide, oxygen and water.

[0076] According to some embodiments of the present invention, the foamed beads are prepared by a foaming process of kettle pressure foaming (reactor immersion foaming method). Extrusion foaming method and compression foaming method are commonly used resin foaming methods. The specific foaming molding process conditions can be conventionally selected in the art. The specific process is known to those skilled in the art and will not be described in detail here.

[0077] According to some embodiments of the present invention, the apparent density of the expanded beads is 60±0.3 g / L, and the apparent density of the expanded beads conventionally selected in the art may include but is not limited to 10-300 g / L. Those skilled in the art are aware of this and will not be elaborated here.

[0078] According to the present invention, the reinforced pre-set material comprises a polypropylene composite material. According to some preferred embodiments of the present invention, the reinforced pre-set material is selected from a polypropylene composite material.

[0079] The position of the reinforcing pre-placed material in the polypropylene foam beads molded body can be selected in a wide range. According to some preferred embodiments of the present invention, the reinforcing pre-placed materials that are farthest apart are respectively located outside the two ends of the polypropylene foam beads molded body; the distance between the reinforcing pre-placed materials inside the molded body is 2-50 mm, preferably 5-25 mm. In this preferred embodiment, the polypropylene foam beads molded body has a more excellent compression strength.

[0080] The conventional apparent density of the expanded beads molded body in the art may include but is not limited to 10-500 g / L, which is known to those skilled in the art and will not be elaborated here. The apparent density of the expanded beads molded body of the present invention is preferably 40±0.3 g / L.

[0081] The specification of the molded body in the present invention is 500mm*500mm*50mm (see the embodiments below), and then cut into different test blocks according to the test conditions.

[0082] The polypropylene foam bead molding of the present invention can improve the compression strength (50%) by ≥50%, preferably ≥100%, compared with the conventional polypropylene foam bead molding of the same base resin, the same shape and the same ratio, while the apparent density, thermal conductivity, molding time and steam pressure are not higher than those of the conventional polypropylene foam bead molding.

[0083] The polypropylene foam bead molded body of the present invention has an apparent density of ≤30%, preferably ≤50%, a thermal conductivity of ≤15%, preferably ≤25%, a molding time of ≤15%, preferably ≤30%, and a steam pressure of ≤10%, preferably ≤25%, compared with other types of reinforced sheet composite polypropylene foam bead molded bodies with the same base resin, the same volume and similar physical properties.

[0084] The second aspect of the present invention is to provide a method for preparing the polypropylene foam beads molded body described in the first aspect, comprising the following steps:

[0085] a. preparing polypropylene foam beads by foaming the components including the raw materials of the polypropylene foam beads material; preferably, firstly, melt-mixing the raw materials including the polypropylene foam beads material except the foaming agent to obtain a polypropylene composition for foam beads, and then mixing the polypropylene composition for foam beads with the foaming agent to obtain polypropylene foam beads by foaming;

[0086] b. Placing the reinforced pre-set material in a mold, and then molding the polypropylene foam beads in the mold to obtain the polypropylene foam beads molded body.

[0087] The position of the reinforcing pre-placed material in the polypropylene foam beads molded body can be selected in a wide range. According to some preferred embodiments of the present invention, the reinforcing pre-placed materials that are farthest apart are respectively located outside the two ends of the polypropylene foam beads molded body; and / or, the distance between the reinforcing pre-placed materials inside the molded body is 2-50 mm, preferably 5-25 mm. In this preferred embodiment, the polypropylene foam beads molded body has a more excellent compression strength.

[0088] Preferably, the amount of the reinforcing pre-placed materials in the present invention can be determined according to the size of the molded body and the preferred distance between the reinforcing pre-placed materials.

[0089] Preferably, the molding conditions include: molding time is not higher than 360s, preferably 330s-360s, and / or steam pressure is not higher than 2.2 bar, for example, 2.0-2.2 bar, preferably not higher than 2.1 bar, and more preferably 2.0-2.1 bar.

[0090] According to the present invention, the temperature conditions during molding are determined by the steam pressure. For example, when the steam pressure is 2.1 bar, the temperature corresponding to the saturated steam is about 135° C. The temperature condition range during molding is not repeated here.

[0091] The molded body of the present invention can be produced in various existing molding machines, and the molds and process conditions used for molding can be conventionally selected in the art, which are known to those skilled in the art and will not be elaborated herein.

[0092] The third aspect of the present invention is to provide an application of the polypropylene foam bead molded body described in the first aspect or the polypropylene foam bead molded body prepared by the preparation method described in the second aspect in materials used in at least one of the following fields: automobiles, communications, aircraft, logistics, insulation, precision machinery and electronic turnover, and packaging.

[0093] Compared with the prior art, the present invention has the following beneficial effects:

[0094] (1) The polypropylene foam beads of the present invention have a compression strength (50%) that is increased by ≥50%, preferably ≥100%, compared with conventional polypropylene foam beads of the same base resin, shape and ratio, while the apparent density, thermal conductivity, molding time and steam pressure are not higher than those of conventional polypropylene foam beads.

[0095] (2) The polypropylene foam bead molding of the present invention has an apparent density of ≤30%, preferably ≤50%, a thermal conductivity of ≤15%, preferably ≤25%, a molding time of ≤15%, preferably ≤30%, and a steam pressure of ≤10%, preferably ≤25%, compared with other types of reinforced sheet composite polypropylene foam bead moldings with the same base resin, the same volume and similar physical properties.

[0096] (3) In the preparation of the polypropylene foam bead molded body provided by the present invention, a high-strength and high-impact polypropylene composite material (preferably a sheet) is pre-placed in a molding mold, and a polypropylene composition that is preferably the same as the sheet matrix resin is subjected to an autoclave foaming process to obtain polypropylene foam beads, which are then subjected to secondary molding in the molding mold to obtain a polypropylene foam bead product.

[0097] (4) Compared with the currently common polypropylene foam beads of the same apparent density, the present invention can significantly improve the physical properties of the product by pre-reinforcing the sheet.

[0098] (5) Compared with the glass fiber nylon composite pre-set sheet or metal sheet reinforced molding used in the currently common composite reinforced polypropylene foam bead molding, the compatibility between the pre-set sheet and the matrix resin is greatly improved, which can effectively reduce the apparent density of the product and improve the thermal insulation performance and production efficiency.

[0099] (6) The polypropylene foam bead molded body of the present invention can be prepared by various existing autoclave foaming and molding processes, and different process methods and different types of foaming agents can be used to prepare polypropylene composition polypropylene foam bead molded bodies with different properties according to the needs of downstream applications.

[0100] (7) The polypropylene foam beads of the present invention are homogeneous components and do not require separation during recycling. They can be directly used in other processing and application fields after crushing, melting and granulation, with lower recycling costs.

[0101] Other features and advantages of the present invention will be described in detail in the following detailed description. DETAILED DESCRIPTION

[0102] The present invention is described in detail below in conjunction with specific embodiments. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the contents of the present invention still fall within the scope of protection of the present invention.

[0104] In the following examples and comparative examples:

[0105] (1) Melt flow rate (MFR): measured according to the method specified in GB / T 3682-2000, wherein for polypropylene (including homopolypropylene, impact copolymer polypropylene and random copolymer polypropylene), the test temperature is 230°C and the load is 2.16 kg; for thermal adhesion enhancers, the test temperature is 190°C and the load is 2.16 kg.

[0106] (2) Molecular weight distribution (Mw / Mn): measured according to the method specified in GB / T 36214.1-2018, where Mw is the weight average molecular weight in g / mol and Mn is the number average molecular weight in g / mol.

[0107] (3) The melting point of the material is determined by the method of GB / T 28724-2012. The sample mass is 5 mg. The temperature is increased from 50°C to 230°C at a rate of 10°C / min, and the temperature is maintained at 230°C for 3 min to eliminate the thermal history. The temperature is then decreased from 230°C to 50°C at a rate of 10°C / min, and the temperature is maintained at 50°C for 1 min. Finally, the temperature is increased from 50°C to 230°C at a rate of 10°C / min. The last temperature increase curve is used to determine the melting point or melting range of the material.

[0108] (4) Sheet tensile strength: measured according to the method specified in GB / T1040.1-2018.

[0109] (5) Drop weight impact strength: measured according to the method specified in GB / T14153-1993.

[0110] (6) Interlayer peel strength: measured according to the method specified in QB / T2358-98.

[0111] The foaming molding performance is tested according to the following method:

[0112] (1) Test method for compressive strength of expanded beads molded body: The compressive strength is measured according to the method specified in GB / T8813.

[0113] (2) Density test method of foamed beads and foamed bead moldings: Measure according to the method described in GB / T 6343.

[0114] (3) Test method for thermal insulation ability of expanded bead molded body: The thermal conductivity is measured according to the method specified in GB / T 10294.

[0115] In the following examples, the β-crystal nucleating agent with the brand name VP101B is sourced from Beijing Research Institute of Chemical Industry of Sinopec Corporation; the sources of some raw materials are described in the examples, and the other raw materials are commercially available unless otherwise specified.

[0116] Example 1

[0117] This example is used to illustrate the preparation of the polypropylene composition, three-layer co-extruded polypropylene sheet, polypropylene fabric, polypropylene composite material, polypropylene composition and polypropylene foamed bead molded body provided by the present invention.

[0118] (1) Preparation of polypropylene composition A:

[0119] Component a is a homopolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, with a melting point of 160°C, a melt flow rate (melt mass flow rate) of 3.2g / 10min, and an isotacticity of 97%; component b is a polypropylene impact copolymer produced by Sinopec Beijing Research Institute of Chemical Industry, with an ethylene content of 11wt%, a melting point of 155°C, and an Izod impact strength of 23KJ / m 2 (23°C), the melt flow rate is 2.0 g / 10 min. The components prepared above are weighed and mixed according to the proportions, wherein the mass fraction Wa of component a is 80 parts by weight, and the mass fraction Wb of component b is 20 parts by weight.

[0120] 0.05 parts by weight of a β-crystal nucleating agent of grade VP101B was added. The mixture was then added to a high-speed stirrer for uniform mixing, and then the mixed material was added to the feeder of a twin-screw extruder manufactured by W&P Company, and the material entered the twin screw through the feeder. During the processing, the temperature of the screw was maintained between 200-230° C. The screw was melt-mixed uniformly, extruded, granulated and dried to obtain a polypropylene composition pellet A. The melting point of the polypropylene composition pellet A was found to be 157° C.

[0121] (2) Polypropylene composition B i Preparation:

[0122] Component x1 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a molecular weight distribution of Mw / Mn of 8.9, a melt flow rate of 8.1 g / 10 min and a melting point of 130°C; component x2 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a molecular weight distribution of Mw / Mn of 7.6, a melt flow rate of 7.2 g / 10 min and a melting point of 135°C; component x3 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a molecular weight distribution of Mw / Mn of 7.3, a melt flow rate of 6.6 g / 10 min and a melting point of 140°C; component y is a polyolefin elastomer with a brand number of 6102, purchased from Exxon, and is an ethylene-propylene copolymer.

[0123] The components prepared above were weighed and mixed according to the proportion, wherein the mass fraction Wxi of component xi was 85 parts by weight, the mass fraction Wy of component y was 15 parts by weight, and the other steps were the same as step (1), and finally a polypropylene composition B was obtained. i Granules (i.e. xi+y=B i , i=1, 2, 3), after testing, the melting point of B1 is 127°C, the melting point of B2 is 132°C, and the melting point of B3 is 138°C.

[0124] (3) Preparation of three-layer co-extruded polypropylene sheet:

[0125] The polypropylene composition A and the polypropylene composition B obtained in the above steps (1) and (2) are i The pellets are dried, and then the polypropylene composition A is added to the core layer extruder of the multi-layer extrusion calendering, and the polypropylene composition B is added to the core layer extruder of the multi-layer extrusion calendering. iAdd to the upper and lower surface extruders of the multi-layer extrusion casting machine. After the pellets are co-extruded and compounded through the extruder die, they pass through the calendering roller and the traction roller in sequence, and then undergo solid phase stretching, trimming and winding to obtain sheets B1AB1, B2AB2, and B3AB3 respectively. Among them, the temperature of the extrusion casting is 230°C, and the temperature of the calendering roller is 58°C. The temperature during the solid phase stretching process is 140°C, the stretching rate is 2m / min, and the stretching ratio is 7 times.

[0126] The composite film (polypropylene sheet) made by stretching and rolling is composed of the upper surface layer (the outer layer of the film B i ), core layer (film A) and lower surface layer (outer film B i The thickness of the composite film is 80 μm, wherein the thickness of the film layer A accounts for 80% of the total thickness of the sheet.

[0127] (4) Preparation of polypropylene fabric:

[0128] The three-layer co-extruded polypropylene sheet obtained in the above step (3) is cut by a high-speed slitting machine with multiple blades to obtain an oriented polypropylene flat ribbon with a width of 3 mm; the oriented flat ribbon is woven by a commercial weaving machine according to the designed fabric structure to obtain plain polypropylene fabrics B1AB1, B2AB2, B3AB3.

[0129] (5) Preparation of polypropylene composite material: The polypropylene fabrics prepared in the above step (4) are stacked in order, from bottom to top, B3AB3, B2AB2, B1AB1, B2AB2, B3AB3, and the total number of stacked layers is 5. The stacked polypropylene fabrics are hot-pressed and fused, and then cooled and shaped to form a polypropylene composite material. The polypropylene fabric is placed at 90° between the warp and the warp. The hot pressing conditions used are: temperature 145°C, hot pressing pressure 5MPa, preheating time 90s, hot pressing time 90s, and cooling time 300s. The thickness of the prepared polypropylene composite material is 391μm.

[0130] According to tests, the drop weight impact strength of the polypropylene composite material is greater than 45 J, the longitudinal tensile strength is greater than 180 MPa, and the interlayer peeling strength is greater than 1.5 N / mm.

[0131] (6) Preparation of polypropylene composition for foamed beads:

[0132] 5 kg of the polypropylene composition A prepared in step (1) and 5 kg of the polypropylene composition B3 prepared in step (2) were added with 30 g of antioxidant 1010, 100 g of 2000 mesh commercial talc as a nucleating agent, and 200 g of commercial graphite color powder, and mixed in a high-speed mixer for 3 minutes. The mixture was extruded and granulated using a twin-screw extruder at a die head temperature of 220° C., a screw speed of 300 rpm, and a torque of 60% to obtain a polypropylene mixture AB.i -1. Its melt mass flow rate MFRB was detected to be 4.9 g / 10 min, and its melting point was 151°C.

[0133] (7) Preparation of polypropylene foam beads

[0134] In a reactor, 100 parts by weight of polypropylene composition resin particles are mixed with 3000 parts by weight of dispersion medium (deionized water), 0.3 parts by weight of surfactant (sodium dodecylbenzene sulfonate), 3 parts by weight of dispersant (kaolin) and 0.2 parts by weight of dispersion enhancer (aluminum sulfate) at one time; the residual air in the reactor is discharged using a carbon dioxide foaming agent, and the reactor cover is tightly closed after the air in the reactor is removed; carbon dioxide is fed into the reactor, and the pressure is initially adjusted until it is stable; then the dispersion in the reactor is stirred and heated at a uniform rate to 1°C lower than the foaming process temperature. Subsequently, the pressure in the reactor is adjusted to the pressure required for foaming; the temperature is raised to the foaming temperature at an average heating rate of 0.1°C / min; under the foaming temperature and pressure conditions, stirring is continued for 0.5 hours. Then, the discharge port of the reactor is opened, and the material in the reactor is discharged into a collection tank to obtain polypropylene foam beads.

[0135] (8) Preparation of polypropylene foam beads

[0136] In a molding machine, the polypropylene composite material obtained in the above step (4) is used as a reinforcing pre-set material. Two square sheets with a side length of 300 mm are hung on the outermost side of the mold, and then four square sheets with a side length of 300 mm are stacked at a spacing of 10 mm and hung in the mold. The polypropylene foam beads obtained in the above step (7) are fed into the molding mold and molded under a certain time and a certain pressure of steam. Subsequently, the obtained molded body is aged for 24 hours under the conditions of a temperature of 100°C and a pressure of standard atmospheric pressure to obtain a polypropylene foam bead molded body. The apparent density, compressive strength (50%) and thermal conductivity are measured, and the molding time and steam pressure are recorded. The results are shown in Table 1.

[0137] Example 2

[0138] This example is used to illustrate the preparation of the polypropylene composition, three-layer co-extruded polypropylene sheet, polypropylene fabric, polypropylene composite material, polypropylene composition and polypropylene foamed bead molded body provided by the present invention.

[0139] (1) Preparation of polypropylene composition A:

[0140] Component a is homopolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, with a melting point of 165°C, a melt flow rate of 8.1g / 10min, and an isotacticity of 97%; component b is a polypropylene impact copolymer produced by Sinopec Beijing Research Institute of Chemical Industry, with an ethylene content of 8wt%, a melting point of 155°C, a melt flow rate of 3.2g / 10min, and an cantilever beam impact strength of 25KJ / m 2 (23°C). The components prepared above were weighed and mixed according to the proportions, wherein the mass fraction Wa of component a was 70 parts by weight, and the mass fraction WB of component b was n The mixture is 30 parts by weight. 0.05 parts by weight of a β-crystal nucleating agent with the grade of VP101B is added. Then the mixture is added to a high-speed stirrer for uniform mixing, and then the mixed material is added to the feeder of a twin-screw extruder manufactured by W&P Company. The material enters the twin screw through the feeder. During the processing, the temperature of the screw is maintained between 200-230°C. The screw is melt-mixed, extruded, granulated and dried to obtain a polypropylene composition pellet A. After testing, the melting point of the polypropylene composition pellet A is 161°C.

[0141] (2) Polypropylene composition B i Preparation:

[0142] Component x1 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a molecular weight distribution Mw / Mn of 8.4, a melting point of 128°C, and a melt flow rate of 7.8 g / 10 min; Component x2 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a molecular weight distribution Mw / Mn of 7.6, a melting point of 134°C, and a melt flow rate of 6.9 g / 10 min; Component x3 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a molecular weight distribution Mw / Mn of 7.1, a melting point of 142°C, and a melt flow rate of 5.2g / 10min; component y is a polyolefin elastomer produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene copolymer with an ethylene content of 15%wt, a melting point of 105°C, and a melt flow rate of 9g / 10min under a load of 2.16kg.

[0143] The components prepared above are weighed and mixed according to the proportion, wherein the mass fraction Wxi of component xi is 80 parts by weight, the mass fraction Wy of component y is 20 parts by weight, and the other steps are the same as step (1), and finally a polypropylene composition B is obtained. i Granules (i.e. xi+y=B i , i=1, 2, 3), after testing, the melting point of B1 is 126°C, the melting point of B2 is 133°C, and the melting point of B3 is 140°C.

[0144] (3) Preparation of three-layer co-extruded polypropylene sheet:

[0145] The preparation process is the same as step (3) of Example 1.

[0146] (4) Preparation of polypropylene fabric:

[0147] The preparation process is the same as step (4) of Example 1.

[0148] (5) Preparation of polypropylene composite materials:

[0149] The preparation process is the same as step (5) of Example 1.

[0150] The thickness of the prepared polypropylene composite material is close to that of Example 1.

[0151] (6) Preparation of polypropylene composition for foamed beads:

[0152] The preparation process is the same as step (6) of Example 1 to obtain a polypropylene mixture AB i ,2, where B i It is B3 in this embodiment. Its melt mass flow rate MFRB is 8.8 g / 10 min and its melting point is 158°C.

[0153] (7) Preparation of polypropylene foam beads

[0154] The preparation process is the same as step (7) of Example 1, except that the polypropylene composition AB prepared in step (6) above is i -2 is the base resin.

[0155] (8) Preparation of polypropylene foam beads

[0156] The preparation process was the same as step (8) of Example 1 to obtain a polypropylene composition autoclave foamed body. The apparent density, compression strength (50%) and thermal conductivity were measured, and the molding time and steam pressure were recorded. The results are shown in Table 1.

[0157] Example 3

[0158] This example is used to illustrate the preparation of the polypropylene composition, three-layer co-extruded polypropylene sheet, polypropylene fabric, polypropylene composite material, polypropylene composition and polypropylene foamed bead molded body provided by the present invention.

[0159] (1) Preparation of polypropylene composition A:

[0160] The preparation process is the same as step (1) of Example 1.

[0161] (2) Polypropylene composition B i Preparation:

[0162] The preparation process is the same as step (2) of Example 1.

[0163] (3) Preparation of three-layer co-extruded polypropylene sheet:

[0164] The main steps are the same as those of Example 1. The thickness of the polypropylene sheet is 80 μm, wherein the thickness of the film layer A accounts for 90% of the total thickness of the sheet.

[0165] (4) Preparation of polypropylene fabric:

[0166] The preparation process is the same as step (4) of Example 1.

[0167] (5) Preparation of polypropylene composite materials:

[0168] The preparation process is the same as step (5) of Example 1.

[0169] The thickness of the prepared polypropylene composite material is close to that of Example 1.

[0170] (6) Preparation of polypropylene composition for foamed beads:

[0171] The preparation process is the same as step (6) of Example 1.

[0172] (7) Preparation of polypropylene foam beads

[0173] The preparation process is the same as step (7) of Example 1.

[0174] (8) Preparation of polypropylene foam beads

[0175] The preparation process was the same as step (8) of Example 1 to obtain a polypropylene composition autoclave foamed body. The apparent density, compression strength (50%) and thermal conductivity were measured, and the molding time and steam pressure were recorded. The results are shown in Table 1.

[0176] Example 4

[0177] This example is used to illustrate the preparation of the polypropylene composition, three-layer co-extruded polypropylene sheet, polypropylene fabric, polypropylene composite material, polypropylene composition and polypropylene foamed bead molded body provided by the present invention.

[0178] (1) Preparation of polypropylene composition A:

[0179] The preparation process is the same as step (1) of Example 1.

[0180] (2) Polypropylene composition B i Preparation:

[0181] The preparation process is the same as step (2) of Example 1.

[0182] (3) Preparation of three-layer co-extruded polypropylene sheet:

[0183] The main preparation process is the same as step (3) of Example 1, wherein the sheet stretching ratio is 10 times.

[0184] (4) Preparation of polypropylene fabric:

[0185] The preparation process is the same as step (4) of Example 1.

[0186] (5) Preparation of polypropylene composite materials:

[0187] The preparation process is the same as step (5) of Example 1.

[0188] The thickness of the prepared polypropylene composite material is close to that of Example 1.

[0189] (6) Preparation of polypropylene composition for foamed beads:

[0190] The preparation process is the same as step (6) of Example 1.

[0191] (7) Preparation of polypropylene foam beads

[0192] The preparation process is the same as step (7) of Example 1.

[0193] (8) Preparation of polypropylene foam beads

[0194] The preparation process was the same as step (8) of Example 1 to obtain a polypropylene composition autoclave foamed body. The apparent density, compression strength (50%) and thermal conductivity were measured, and the molding time and steam pressure were recorded. The results are shown in Table 1.

[0195] Example 5

[0196] This example is used to illustrate the preparation of the polypropylene composition, three-layer co-extruded polypropylene sheet, polypropylene fabric, polypropylene composite material, polypropylene composition and polypropylene foamed bead molded body provided by the present invention.

[0197] (1) Preparation of polypropylene composition A:

[0198] The preparation process is the same as step (1) of Example 1.

[0199] (2) Polypropylene composition B i Preparation:

[0200] The preparation process is the same as step (2) of Example 1.

[0201] (3) Preparation of three-layer co-extruded polypropylene sheet:

[0202] The preparation process is the same as step (3) of Example 1.

[0203] (4) Preparation of polypropylene fabric:

[0204] The preparation process is the same as step (4) of Example 1.

[0205] (5) Preparation of polypropylene composite materials:

[0206] The main steps are the same as those in Example 1. The laminated polypropylene sheet includes two layers of polypropylene fabric (B3AB3). The hot pressing conditions are: temperature 140°C, hot pressing pressure 2MPa, preheating time 120s, hot pressing time 10s, cooling time 300s. The thickness of the prepared polypropylene composite material is 128μm.

[0207] (6) Preparation of polypropylene composition for foamed beads:

[0208] The preparation process is the same as step (6) of Example 1.

[0209] (7) Preparation of polypropylene foam beads

[0210] The preparation process is the same as step (7) of Example 1.

[0211] (8) Preparation of polypropylene foam beads

[0212] The preparation process was the same as step (8) of Example 1 to obtain a polypropylene composition autoclave foamed body. The apparent density, compression strength (50%) and thermal conductivity were measured, and the molding time and steam pressure were recorded. The results are shown in Table 1.

[0213] Example 6

[0214] This example is used to illustrate the preparation of the polypropylene composition, three-layer co-extruded polypropylene sheet, polypropylene fabric, polypropylene composite material, polypropylene composition and polypropylene foamed bead molded body provided by the present invention.

[0215] (1) Preparation of polypropylene composition A:

[0216] The preparation process is the same as step (1) of Example 1.

[0217] (2) Polypropylene composition B i Preparation:

[0218] The preparation process is the same as step (2) of Example 1.

[0219] (3) Preparation of three-layer co-extruded polypropylene sheet:

[0220] The preparation process is the same as step (3) of Example 1.

[0221] (4) Preparation of polypropylene composite materials:

[0222] The polypropylene fabric was not prepared, but the three-layer co-extruded polypropylene sheet prepared in step (3) was used to replace the polypropylene fabric obtained in step (4) of Example 1, and the laminated and hot-pressed layers were sequentially stacked according to step (5) of Example 1. The thickness of the prepared polypropylene composite material was 0.39 mm.

[0223] (5) Preparation of polypropylene composition for foamed beads:

[0224] The preparation process is the same as step (6) of Example 1.

[0225] (6) Preparation of polypropylene foam beads

[0226] The preparation process is the same as step (7) of Example 1.

[0227] (7) Preparation of polypropylene foam beads

[0228] The preparation process was the same as step (8) of Example 1 to obtain a polypropylene composition autoclave foamed body. The apparent density, compression strength (50%) and thermal conductivity were measured, and the molding time and steam pressure were recorded. The results are shown in Table 1.

[0229] Example 7

[0230] This example is used to illustrate the preparation of the polypropylene composition, three-layer co-extruded polypropylene sheet, polypropylene fabric, polypropylene composite material, polypropylene composition and polypropylene foamed bead molded body provided by the present invention.

[0231] (1) Preparation of polypropylene composition A:

[0232] The preparation process is the same as step (1) of Example 1.

[0233] (2) Polypropylene composition B i Preparation:

[0234] The preparation process is the same as step (2) of Example 1.

[0235] (3) Preparation of three-layer co-extruded polypropylene sheet:

[0236] The preparation process is the same as step (3) of Example 1.

[0237] (4) Preparation of polypropylene fabric:

[0238] The preparation process is the same as step (4) of Example 1.

[0239] (5) Preparation of polypropylene composite materials:

[0240] The preparation process is the same as step (5) of Example 1.

[0241] The thickness of the prepared polypropylene composite material is close to that of Example 1.

[0242] (6) Preparation of polypropylene composition for foamed beads:

[0243] The preparation process is the same as step (6) of Example 1. The preparation process is the same as step (6) of Example 1, except that 9.5 kg of the polypropylene composition A prepared in step (1) and 0.5 kg of the polypropylene composition B3 pellets prepared in step (2) are taken. The melt mass flow rate MFRA is 4.6 g / 10 min; the polypropylene composition AB is i The melting point of -3 is 157°C.

[0244] (7) Preparation of polypropylene foam beads

[0245] The preparation process is the same as step (7) of Example 1.

[0246] (8) Preparation of polypropylene foam beads

[0247] The preparation process was the same as step (8) of Example 1 to obtain a polypropylene composition autoclave foamed body. The apparent density, compression strength (50%) and thermal conductivity were measured, and the molding time and steam pressure were recorded. The results are shown in Table 1.

[0248] Example 8

[0249] This example is used to illustrate the preparation of the polypropylene composition, three-layer co-extruded polypropylene sheet, polypropylene fabric, polypropylene composite material, polypropylene composition and polypropylene foamed bead molded body provided by the present invention.

[0250] (1) Preparation of polypropylene composition A:

[0251] The preparation process is the same as step (1) of Example 1.

[0252] (2) Polypropylene composition B i Preparation:

[0253] The preparation process is the same as step (2) of Example 1.

[0254] (3) Preparation of three-layer co-extruded polypropylene sheet:

[0255] The preparation process is the same as step (3) of Example 1.

[0256] (4) Preparation of polypropylene fabric:

[0257] The preparation process is the same as step (4) of Example 1.

[0258] (5) Preparation of polypropylene composite materials:

[0259] The preparation process is the same as step (5) of Example 1.

[0260] The thickness of the prepared polypropylene composite material is close to that of Example 1.

[0261] (6) Preparation of polypropylene composition for foamed beads:

[0262] The preparation process is the same as step (6) of Example 1, except that 0.5 kg of the polypropylene composition A prepared in step (1) and 9.5 kg of the polypropylene composition B3 pellets prepared in step (2) are taken. The melt mass flow rate MFR is 5.2 g / 10 min, and the polypropylene composition AB is i The melting point of -4 is 138°C.

[0263] (7) Preparation of polypropylene foam beads

[0264] The preparation process is the same as step (7) of Example 1.

[0265] (8) Preparation of polypropylene foam beads

[0266] The preparation process was the same as step (8) of Example 1 to obtain a polypropylene composition autoclave foamed body. The apparent density, compression strength (50%) and thermal conductivity were measured, and the molding time and steam pressure were recorded. The results are shown in Table 1.

[0267] Example 9

[0268] This example is used to illustrate the preparation of the polypropylene composition, three-layer co-extruded polypropylene sheet, polypropylene fabric, polypropylene composite material, polypropylene composition and polypropylene foamed bead molded body provided by the present invention.

[0269] (1) Preparation of polypropylene composition A:

[0270] The preparation process is the same as step (1) of Example 1.

[0271] (2) Polypropylene composition B i Preparation:

[0272] The preparation process is the same as step (2) of Example 1.

[0273] (3) Preparation of three-layer co-extruded polypropylene sheet:

[0274] The preparation process is the same as step (3) of Example 1.

[0275] (4) Preparation of polypropylene fabric:

[0276] The preparation process is the same as step (4) of Example 1.

[0277] (5) Preparation of polypropylene composite materials:

[0278] The preparation process is the same as step (5) of Example 1.

[0279] The thickness of the prepared polypropylene composite material is close to that of Example 1.

[0280] (6) Preparation of polypropylene composition for foamed beads:

[0281] The preparation process is the same as step (6) of Example 1.

[0282] (7) Preparation of polypropylene foam beads

[0283] The preparation process is the same as step (7) of Example 1.

[0284] (8) Preparation of polypropylene foam beads

[0285] The preparation process is the same as step (8) of Example 1, except that two square sheets with a side length of 300 mm are stacked and hung at a distance of 12.5 mm in the middle of the mold to obtain a polypropylene composition autoclave foaming molding. The apparent density, compression strength (50%) and thermal conductivity are measured, and the molding time and steam pressure are recorded. The results are shown in Table 1.

[0286] Example 10

[0287] This example is used to illustrate the preparation of the polypropylene composition, three-layer co-extruded polypropylene sheet, polypropylene fabric, polypropylene composite material, polypropylene composition and polypropylene foamed bead molded body provided by the present invention.

[0288] (1) Preparation of polypropylene composition A:

[0289] The preparation process is the same as step (1) of Example 1.

[0290] (2) Polypropylene composition B i Preparation:

[0291] The preparation process is the same as step (2) of Example 1.

[0292] (3) Preparation of three-layer co-extruded polypropylene sheet:

[0293] The preparation process is the same as step (3) of Example 1.

[0294] (4) Preparation of polypropylene fabric:

[0295] The preparation process is the same as step (4) of Example 1.

[0296] (5) Preparation of polypropylene composite materials:

[0297] The preparation process is the same as step (5) of Example 1.

[0298] The thickness of the prepared polypropylene composite material is close to that of Example 1.

[0299] (6) Preparation of polypropylene composition for foamed beads:

[0300] The preparation process is the same as step (6) of Example 1.

[0301] (7) Preparation of polypropylene foam beads

[0302] The preparation process is the same as step (7) of Example 1.

[0303] (8) Preparation of polypropylene foam beads

[0304] The preparation process is the same as step (8) of Example 1, except that 19 square sheets with a side length of 300 mm are stacked at a spacing of 2.5 mm and then hung to obtain a polypropylene composition autoclave foaming molding. The apparent density, compression strength (50%) and thermal conductivity were measured, and the molding time and steam pressure were recorded. The results are shown in Table 1.

[0305] Comparative Example 1

[0306] A three-layer coextruded polypropylene sheet was prepared according to the method of Example 1, except that only the polypropylene composition A was used for extrusion casting into a single-layer film with a thickness of 80 μm.

[0307] Polypropylene fabric and polypropylene composite material were prepared according to the method of Example 1. The thickness of the prepared polypropylene composite material was close to that of Example 1.

[0308] The preparation process of the polypropylene composition for foamed beads is the same as step (6) of Example 1, except that only the polypropylene composition A is used. The preparation process of the polypropylene foamed beads is the same as step (7) of Example 1. The preparation process of the polypropylene foamed beads molded body is the same as step (8) of Example 1 to obtain a polypropylene composition autoclave foamed molded body. The apparent density, compressive strength (50%) and thermal conductivity were measured, and the molding time and steam pressure were recorded. The results are shown in Table 1.

[0309] Comparative Example 2

[0310] A three-layer coextruded polypropylene sheet was prepared according to the method of Example 1, except that only the polypropylene composition B3 was used for extrusion casting into a single-layer film with a thickness of 80 μm.

[0311] Polypropylene fabric and polypropylene composite material were prepared according to the method of Example 1. The thickness of the prepared polypropylene composite material was close to that of Example 1.

[0312] The preparation process of the polypropylene composition for foam beads is the same as step (6) of Example 1, except that only the polypropylene composition B3 is used, the preparation process of the polypropylene foam beads is the same as step (7) of Example 1, and the preparation process of the polypropylene foam beads molded body is the same as step (8) of Example 1, to obtain a polypropylene composition autoclave foamed molded body. The apparent density, compressive strength (50%) and thermal conductivity were measured, and the molding time and steam pressure were recorded. The results are shown in Table 1.

[0313] Comparative Example 3

[0314] A three-layer coextruded polypropylene sheet was prepared according to the method of Example 1, except that the polypropylene composition A contained only component b.

[0315] Polypropylene fabric and polypropylene composite material were prepared according to the method of Example 1. The thickness of the prepared polypropylene composite material was close to that of Example 1.

[0316] The preparation process of the polypropylene composition for foaming beads is the same as step (6) of Example 1, except that only component b is used in the polypropylene composition A. The preparation process of polypropylene foaming beads is the same as step (7) of Example 1, and the preparation process of the polypropylene foaming bead molded body is the same as step (8) of Example 1, to obtain a polypropylene composition autoclave foaming molded body. The apparent density, compression strength (50%) and thermal conductivity were measured, and the molding time and steam pressure were recorded. The results are shown in Table 1.

[0317] Comparative Example 4

[0318] A three-layer coextruded polypropylene sheet was prepared according to the method of Example 1. i Contains only component y.

[0319] Polypropylene fabric and polypropylene composite material were prepared according to the method of Example 1. The thickness of the prepared polypropylene composite material was close to that of Example 1.

[0320] The preparation process of the polypropylene composition for foaming beads is the same as step (6) of Example 1, except that the polypropylene composition B i The polypropylene foam beads are prepared in the same manner as step (7) of Example 1, and the polypropylene foam beads molded body is prepared in the same manner as step (8) of Example 1 to obtain a polypropylene composition autoclave foamed molded body. The apparent density, compression strength (50%) and thermal conductivity are measured, and the molding time and steam pressure are recorded. The results are shown in Table 1.

[0321] Comparative Example 5

[0322] A three-layer co-extruded polypropylene sheet, a polypropylene fabric, and a polypropylene composite material were prepared according to the method of Example 1. The thickness of the prepared polypropylene composite material was close to that of Example 1.

[0323] A coextruded polypropylene sheet was prepared according to the method of Example 6, except that component B i The materials are selected in the following manner: component x1 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 140°C; component x2 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 135°C; component x3 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 130°C; the melt flow rates of components x1-x3 are all 2-10g / 10min.

[0324] Finally, the polypropylene composition B is obtained. i Granules (i.e. x i +y=B i , i=1, 2, 3), after testing, the melting point of B1 is 138°C, the melting point of B2 is 132°C, and the melting point of B3 is 127°C.

[0325] A polypropylene fabric and a polypropylene composite material were prepared according to the method of Example 1. The thickness of the prepared polypropylene composite material was close to that of Example 6.

[0326] The preparation process of the polypropylene composition for foam beads is the same as step (6) of Example 1, the preparation process of the polypropylene foam beads is the same as step (7) of Example 1, and the preparation process of the polypropylene foam beads molded body is the same as step (8) of Example 1, to obtain a polypropylene composition autoclave foamed molded body. The apparent density, compressive strength (50%) and thermal conductivity were measured, and the molding time and steam pressure were recorded. The results are shown in Table 1.

[0327] Comparative Example 6

[0328] The preparation process of the polypropylene composition for foam beads is the same as step (6) of Example 1, the preparation process of the polypropylene foam beads is the same as step (7) of Example 1, and the preparation process of the polypropylene foam bead molded body is the same as step (8) of Example 1, except that no sheet is hung inside the mold. The polypropylene composition autoclave foamed molded body is obtained. The apparent density, compression strength (50%) and thermal conductivity are measured, and the molding time and steam pressure are recorded. The results are shown in Table 1.

[0329] Comparative Example 7

[0330] A three-layer co-extruded polypropylene sheet, a polypropylene fabric, and a polypropylene composite material were prepared according to the method of Example 1. The thickness of the prepared polypropylene composite material was close to that of Example 1.

[0331] The preparation process of the polypropylene composition for foam beads is the same as step (6) of Example 1, the preparation process of polypropylene foam beads is the same as step (7) of Example 1, and the preparation process of the polypropylene foam bead molded body is the same as step (8) of Example 1, except that 49 square sheets with a side length of 300 mm were stacked and hung in the middle of the mold with a spacing of 1 mm, and the molding failed.

[0332] Comparative Example 8

[0333] A three-layer co-extruded polypropylene sheet, a polypropylene fabric, and a polypropylene composite material were prepared according to the method of Example 1. The thickness of the prepared polypropylene composite material was close to that of Example 1.

[0334] The preparation process of the polypropylene composition for foam beads is the same as step (6) of Example 1, the preparation process of the polypropylene foam beads is the same as step (7) of Example 1, and the preparation process of the polypropylene foam beads molded body is the same as step (8) of Example 1, except that 5 square glass fiber composite sheets with a side length of 300 mm and a thickness of 1.7 mm purchased from the market are stacked and hung in the middle of the mold to obtain a polypropylene composition autoclave foamed molded body. The apparent density, compressive strength (50%) and thermal conductivity were measured, and the molding time and steam pressure were recorded. The results are shown in Table 1.

[0335] Comparative Example 9

[0336] A three-layer co-extruded polypropylene sheet, a polypropylene fabric, and a polypropylene composite material were prepared according to the method of Example 1. The thickness of the prepared polypropylene composite material was close to that of Example 1.

[0337] The preparation process of the polypropylene composition for foam beads is the same as step (6) of Example 1, the preparation process of the polypropylene foam beads is the same as step (7) of Example 1, and the preparation process of the polypropylene foam beads molded body is the same as step (8) of Example 1, except that a stainless steel sheet with a side length of 300 mm and a thickness of 2.5 mm purchased from the market is hung in the middle of the mold to obtain a polypropylene composition autoclave foamed molded body. The apparent density, compressive strength (50%) and thermal conductivity were measured, and the molding time and steam pressure were recorded. The results are shown in Table 1.

[0338] Experimental example

[0339] The polypropylene composite materials and polypropylene foam beads molded bodies obtained in the above examples and comparative examples were tested according to the following methods. The test results are shown in Table 1.

[0340] (1) The compressive strength of the expanded beads molded body was prepared and measured according to the method specified in GB / T8813.

[0341] (2) The apparent density of the expanded beads molded body was prepared and measured according to the method specified in GB / T 6343.

[0342] (3) The thermal conductivity of the expanded beads molded body was prepared and measured according to the method specified in GB / T 10294.

[0343] Table 1

[0344]

[0345]

[0346] From the results of the examples, it can be seen that the polypropylene composite material prepared according to the present invention has both good tensile properties and impact resistance, and also has good interlayer peeling strength at a relatively low hot pressing temperature. From Examples 7 and 8, it can be seen that the polypropylene composition A and B of the foamed bead matrix resin are regulated. i The ratio has no significant effect on the performance of the final product.

[0347] Compared with Comparative Example 6, the foamed bead molded body prepared with this as the reinforcement sheet can significantly improve the compression strength at a similar or even slightly lower apparent density than the foamed bead molded body prepared by the conventional process without reducing its thermal insulation ability and production efficiency.

[0348] From Comparative Examples 1-4, it can be seen that only using a single-layer sheet structure, a single polymer component, or using an interlayer ratio outside the scope of the embodiment will lead to a decrease in the performance of the laminated polypropylene sheet or fabric, thereby causing a decrease in the compression strength, heat insulation capacity and production efficiency of the final foamed bead molded body. Comparative Example 5 verifies that the melting point does not follow the gradient in this application and the inventive effect cannot be achieved.

[0349] It can be seen from Example 9, Example 10 and Comparative Example 7 that the distance between the polypropylene composite material reinforced sheets has a significant impact on the final product. As the distance between the sheets decreases, that is, the number of sheets in the molded body increases, the physical properties improve and the production efficiency decreases. When the distance between the sheets is too short, it is difficult to obtain a foamed product of qualified quality.

[0350] It can be seen from Comparative Examples 8 and 9 that although the use of commonly used sheet reinforcement methods such as glass fiber and metal in the industry can also increase the compressive strength of the foamed bead molding to the level of the embodiments, the apparent density and thermal conductivity of the product will greatly exceed that of Comparative Example 6, and the production efficiency will also be greatly reduced.

[0351] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.

[0352] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

Claims

1. A polypropylene foam bead molded body, comprising a plurality of reinforced pre-set materials and a polypropylene foam bead material bonded to the reinforced pre-set materials by molding, wherein the reinforced pre-set materials comprise a polypropylene composite material; The polypropylene composite material comprises a plurality of polypropylene sheet unit groups stacked in sequence; each polypropylene sheet unit group comprises at least one identical or different polypropylene sheet unit, and each polypropylene sheet unit comprises a core layer A i and located in the core layer A i The outer layer B on both sides i , B' i , structure B i A i B' i The structure of the polypropylene composite material is, from bottom to top, the nth group... the ith group... the second group, the first group, the second group... the ith group... the nth group, and the total number of stacked groups of polypropylene sheet unit groups is 2n-1; i and n are both integers not less than 2, and i≤n; in, Core layer A in polypropylene sheet unit i Containing polypropylene composition A i , outer layer B i With outer layer B' i The same or different, each corresponding to a polypropylene composition B i , polypropylene composition B' i , The polypropylene composition A i The melting point is greater than that of the polypropylene composition B i , the polypropylene composition B' i The average melting point of all outer layers in the i-th group is greater than or equal to the average melting point of all outer layers in the i-1-th group.

2. The polypropylene foam beads molded body according to claim 1, characterized in that: Polypropylene composition A i Melting point and polypropylene composition B i The difference in melting points, polypropylene composition A i The melting point of polypropylene composition B' i The difference in melting points of each is greater than or equal to 5°C, preferably greater than or equal to 10°C, more preferably greater than or equal to 20°C; and / or, The difference between the average melting point of all outer layers in the i-th group and the average melting point of all outer layers in the i-1-th group is the same or different, and is each 1-40°C, preferably 1-10°C, more preferably 1-5°C.

3. The polypropylene foam beads molded body according to claim 1, characterized in that: 2≤n≤100, preferably, 2≤n≤50; and / or, Each group of polypropylene ply units, independently of one another, comprises 1 to 10, preferably 1 to 5, identical or different polypropylene ply units.

4. The polypropylene foam beads molded body according to claim 1, characterized in that: Based on the total thickness of each polypropylene sheet unit, the core layer A in each polypropylene sheet unit is i The thickness of the composite film accounts for 51%-89% of the total thickness, preferably 71%-89%, and more preferably 71%-80%.

5. The polypropylene foam beads molded body according to claim 1, characterized in that: The polypropylene composition A i Including one or more of homopolymer polypropylene, random copolymer polypropylene and impact copolymer polypropylene; and / or, The polypropylene composition B i , B' i Each comprises one or more of homopolymer polypropylene, random copolymer polypropylene and impact copolymer polypropylene; preferably the polypropylene composition B i and / or polypropylene composition B' i Also contains thermal bonding enhancer i .

6. The polypropylene foam beads molded body according to claim 1, characterized in that: Polypropylene composition A i Including homopolymer polypropylene i and impact copolymer polypropylene b i ; Preferably, the polypropylene composition A i Based on the total weight of i Comprising 50-99wt% homopolymer polypropylene a i , 1-50wt% impact copolymer polypropylene b i ; Further preferably, the polypropylene composition A i Including 70-90wt% homopolymer polypropylene a i , 10-30wt% impact copolymer polypropylene b i and / or, The polypropylene composition B i , the polypropylene composition B' i Each comprising random copolymer polypropylene x i and thermal bonding enhancers i ; Preferably, the polypropylene composition B i , the polypropylene composition B' i Based on the total weight of each, the polypropylene composition B i , the polypropylene composition B' i Each comprising 70-99 wt% of random copolymer polypropylene x i , 1-30wt% thermal bonding enhancer i ; Further preferably, the polypropylene composition B i , the polypropylene composition B' i Each comprising 80-90 wt% of random copolymer polypropylene x i , 10-20wt% thermal bonding enhancer i .

7. The polypropylene foam beads molded body according to claim 6, characterized in that: The homopolymer polypropylene a i have: The melting point is 150-170°C, preferably 160-170°C; and / or, The melt flow rate at 230°C and 2.16 kg load is 0.5-50 g / 10 min, preferably 1-20 g / 10 min, and more preferably 2.5-18 g / 10 min; and / or, The isotacticity (mm) is not less than 96%.

8. The polypropylene foam beads molded body according to claim 6, characterized in that: The impact copolymer polypropylene b i The melting point is 150-170°C: and / or, The impact copolymer polypropylene b i The monomer copolymerized with propylene is ethylene or butene, preferably butene; and / or, The impact copolymer polypropylene b i The melt flow rate at 230°C and 2.16 kg load is 0.5-50 g / 10 min, preferably 1-20 g / 10 min, and more preferably 2.5-18 g / 10 min; and / or, The impact copolymer polypropylene b i The cantilever beam impact strength is not less than 20KJ / m 2 .

9. The polypropylene foam beads molded body according to claim 6, characterized in that: The random copolymer polypropylene x i have: The melting point is 110-150°C, preferably 120-140°C; and / or, The melt flow rate at 230°C and 2.16 kg load is 0.5-50 g / 10 min, preferably 1-20 g / 10 min, and more preferably 3-18 g / 10 min; and / or, The molecular weight distribution Mw / Mn is 5-12, preferably 7-10; and / or, It is a copolymer of propylene and ethylene and / or butene, preferably an ethylene-propylene-butene terpolymer and / or a propylene-ethylene binary copolymer.

10. The polypropylene foam beads molded body according to claim 6, characterized in that: The thermal bonding enhancer i have: The melting point or viscosity flow temperature is 70-110°C; and / or, The melt flow rate at 190°C and 2.16 kg load is 0.5-50 g / 10 min, preferably 1-20 g / 10 min, and more preferably 1-18 g / 10 min; and / or, One or more selected from polyolefin elastomer, EPDM rubber, SEBS, SBS, EVA, and petroleum resin; preferably, polyolefin elastomer and / or petroleum resin.

11. The polypropylene foam beads molded body according to claim 10, characterized in that: The polyolefin elastomer is a copolymer elastomer of ethylene and propylene and / or alpha olefin, wherein the alpha olefin is preferably a C4-C12 alpha olefin, more preferably 1-butene and / or 1-octene; and / or, The petroleum resin is a C5 and / or C9 hydrogenated petroleum resin with a softening point of 100-150° C. and is preferably a cyclopentadiene type resin.

12. The polypropylene foam beads molded body according to claim 1, characterized in that: The core layer A i It also contains a β-crystal nucleating agent; preferably, The β-crystal nucleating agent is at least one selected from the group consisting of condensed aromatic hydrocarbons, group IIA two-component complexes, aromatic diamides, rare earth compounds and cyclic dicarboxylates; and / or, The polypropylene composition A i The total amount is 100 parts by weight, the core layer A i The content of the β-crystal nucleating agent is 0.01-0.5 parts by weight.

13. The polypropylene foam beads molded body according to any one of claims 1 to 12, characterized in that: The polypropylene sheet unit is a polypropylene sheet and / or a polypropylene fabric; preferably, the polypropylene sheet unit is a polypropylene sheet or a polypropylene fabric; more preferably, The polypropylene sheet comprises a polypropylene composition A i , polypropylene composition B i , polypropylene composition B' i The components are co-extruded; and / or The polypropylene fabric is prepared by the following method: firstly i , polypropylene composition B i , polypropylene composition B' i The inner components are co-extruded to obtain a polypropylene sheet, and the polypropylene sheet is then woven to obtain the polypropylene fabric; preferably, the polypropylene fabric has a three-dimensional structure of plain, twill and / or satin; more preferably, The polypropylene sheet units are connected by heat-compression bonding.

14. The polypropylene foam beads molded body according to any one of claims 1 to 12, characterized in that: The polypropylene foamed beads material contains the polypropylene composition A i At least one of and / or the polypropylene composition B i , the polypropylene composition B' i At least one of, and optional auxiliary agents; preferably, The auxiliary agent is selected from one or more of antioxidants, antistatic agents, lubricants, anti-aging agents, flame retardants, and toners; and / or, The polypropylene foam bead material contains a foaming agent and / or is foamed by an inorganic physical foaming agent; preferably, the inorganic physical foaming agent is selected from at least one of air, nitrogen, carbon dioxide, oxygen and water; and / or, the foaming agent is selected from a chemical foaming agent and / or an organic physical foaming agent; more preferably, the chemical foaming agent is selected from at least one of azodicarbonamide, p-toluenesulfonyl hydrazide, semicarbazides, tetrazoles, sodium bicarbonate and sodium citrate; the organic physical foaming agent is selected from at least one of an aliphatic hydrocarbon foaming agent, an alicyclic hydrocarbon foaming agent, and a halogenated hydrocarbon foaming agent.

15. The polypropylene foam beads molded body according to any one of claims 1 to 12, characterized in that: The reinforced prefabricated material is selected from a polypropylene composite material; and / or, The reinforced pre-set materials which are farthest apart are respectively located outside the two ends of the polypropylene foamed bead molded body; The distance between the reinforcing pre-placed materials inside the formed body is 2-50 mm, preferably 5-25 mm.

16. A method for preparing the polypropylene foam beads molded body according to any one of claims 1 to 15, comprising the following steps: a. preparing polypropylene foam beads by foaming the components including the raw materials of the polypropylene foam beads material; preferably, firstly melt-mixing the raw materials including the polypropylene foam beads material except the foaming agent to obtain a polypropylene composition for foam beads, and then mixing the polypropylene composition for foam beads with the foaming agent to obtain polypropylene foam beads by foaming; b. Placing the reinforced pre-set material in a mold, and then molding the polypropylene foam beads in the mold to obtain the polypropylene foam beads molded body.

17. Use of the polypropylene foam beads molded body according to any one of claims 1 to 15 or the polypropylene foam beads molded body prepared by the preparation method described in claim 16 in materials used in at least one of the following fields: automobiles, communications, aircraft, logistics, thermal insulation, precision machinery and electronic turnover, and packaging.