Green conveyor belt cover rubber and preparation method thereof
By replacing carbon black with high dispersion white carbon black and silane coupling agent in the conveyor belt, the problem of difficult to achieve the rolling resistance and power consumption reduction of green conveyor belts in the prior art is solved, and the goal of green manufacturing and use is achieved, and the improvement of the goal of improving The wear resistance and environmental performance of the product.
Patent Information
- Application Number
- CN202411172006.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-08
AI Technical Summary
The existing conveyor belt technology has failed to realize the concept of green conveyor belts, cannot reduce rolling resistance and power consumption without losing performance, and has failed to meet the requirements of energy conservation, environmental protection and carbon reduction.
Replace most of the carbon black with new high-dispersible white carbon black dispersion additives and silane coupling agents. By improving the dispersion and processing performance of white carbon black, the electric energy consumption of the mixing glue is reduced, and dust and smoke are reduced. Emissions to achieve energy-saving, environmentally friendly and carbon reduction production processes.
It effectively reduces the power consumption of the mixed rubber, reduces dust and flue gas emissions, improves the wear resistance and weather resistance of the product, and realizes the production and use requirements of green conveyor belts.
Smart Images

Figure BDA0005009556330000171
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of rubber, in particular to a green conveyor belt covering rubber and a preparation method thereof. Background Art
[0002] At present, no scientific research unit or conveyor belt production unit in China has proposed the concept of "green conveyor belt". Low rolling resistance conveyor belts and energy-saving and environmentally friendly conveyor belts have been proposed, and there are also related papers and patents, but these cannot meet the requirements of "green conveyor belts".
[0003] Green conveyor belt means that without losing the performance of the conveyor belt, the rolling resistance of the conveyor belt is reduced by 10-20% and the power consumption is reduced by more than 5% compared with ordinary conveyor belts through the application and design of new materials, which effectively reduces energy consumption and carbon dioxide emissions. With the implementation of the EU labeling law, people's attention to green conveyor belts has gradually increased.
[0004] Green conveyor belt refers to a conveyor belt product that is energy-saving, environmentally friendly, and carbon-reducing during production and use. The entire production process implements the concept of green manufacturing, and the application process advocates green use. Green conveyor belts have low running resistance, low power consumption, and low carbon emissions. The manufacture of green conveyor belts must meet the following overall requirements: 1. Use environmentally friendly, non-toxic and harmless raw materials that meet the EU REACH environmental standards; 2. The production process achieves low energy consumption, low noise, low dust, and low smoke; 3. The product has energy-saving, safety, and environmental protection requirements. The development of the formula and preparation process of green conveyor belts that meet the above requirements is the focus of research in this field at this stage. Summary of the invention
[0005] The purpose of the present invention is to provide a green conveyor belt covering rubber and a preparation method thereof to solve the problems existing in the above-mentioned prior art. The present invention adopts a new type of highly dispersed white carbon black plus a white carbon black dispersing aid and a coupling agent to replace most of the carbon black, thereby reducing energy consumption, dust, and smoke during the production and use of the conveyor belt, truly realizing green production of energy saving, consumption reduction, and carbon reduction, making the conveyor belt energy-saving, safe, carbon-reducing, and environmentally friendly.
[0006] To achieve the above object, the present invention provides the following solutions:
[0007] One of the technical solutions of the present invention: a green conveyor belt covering rubber, the raw materials of which include the following components by weight:
[0008] 100 parts of raw rubber;
[0009] Naphthenic oil 0-30 parts;
[0010] 20-80 parts of carbon black;
[0011] 20-80 parts of white carbon black;
[0012] 3-5 parts of white carbon black dispersant;
[0013] Silane coupling agent 2-15 parts;
[0014] 0.3 to 5 parts of accelerator or cross-linking agent;
[0015] 0.2-3 parts of vulcanizing agent;
[0016] 1-5 parts of zinc oxide;
[0017] 1-5 parts of stearic acid;
[0018] Paraffin 0-5 parts;
[0019] 1 to 4 parts of antioxidant.
[0020] Furthermore, the raw rubber includes one or more of natural rubber (NR), styrene-butadiene rubber (SBR), butadiene rubber (BR), and ethylene-propylene rubber (EPR); the antioxidant includes one or more of antioxidant RD, antioxidant D, antioxidant 4020, antioxidant H, antioxidant DPD, antioxidant 264, and antioxidant MB; the accelerator includes one or more of accelerator M, accelerator DM, accelerator NS, accelerator D, accelerator DPG, and accelerator MBTS; and the co-crosslinking agent includes TAIC.
[0021] Ethylene-propylene rubber is a synthetic rubber with ethylene and propylene as the main monomers. According to the different monomer compositions in the molecular chain, it can be divided into EPDM and EPDM. The former is a copolymer of ethylene and propylene, represented by EPM, and the latter is a copolymer of ethylene, propylene and a small amount of a third non-conjugated diene monomer, represented by EPDM. Both are collectively referred to as ethylene-propylene rubber (EPR).
[0022] Furthermore, the carbon black includes one or more of N220, N234, N330, N375, N339, N650, and N660.
[0023] Furthermore, the white carbon black is highly dispersed nano white carbon black, the DBP absorption is 165-200 ml / 100 g, and the CTAB specific surface area is 150-180 m 2 / g.
[0024] Furthermore, the raw materials of the white carbon black dispersant include the following components by weight: 20-30 parts of C8-C22 fatty acid, 5-10 parts of protective wax, 3-6 parts of fatty acid ester, 1-2 parts of antioxidant, 2-5 parts of calcium carbonate and 1-3 parts of zinc oxide.
[0025] Silica dispersant can improve the processing performance of silica filled rubber, increase mixing efficiency, reduce mixing energy consumption, and improve the dispersibility of silica.
[0026] This silica dispersant is suitable for dispersing light-colored fillers, especially for rubber compounds with high silica filling content. It can quickly reduce Mooney viscosity, shorten mixing time, significantly improve the processing performance of rubber compounds, and improve processing efficiency. It has no effect on the vulcanization process, but can improve the flow of rubber compounds and the surface appearance of rubber compounds.
[0027] Furthermore, the protective wax includes paraffin wax, microcrystalline wax or PE wax.
[0028] Furthermore, the fatty acid ester includes polyethylene glycol fatty acid ester.
[0029] Furthermore, the antioxidant includes the antioxidant BHT (butylated hydroxytoluene).
[0030] Furthermore, the preparation method of the white carbon black dispersant is: placing a C8-C22 fatty acid in a reactor, stirring and heating at 100-110°C, then adding protective wax and fatty acid ester, and continuing to stir for 10-15 minutes after the materials are completely melted, adding an antioxidant, calcium carbonate and zinc oxide and continuing to stir for 10-15 minutes, cooling to room temperature, discharging the materials, and crushing to obtain the white carbon black dispersant.
[0031] Furthermore, the vulcanizing agent and the silane coupling agent are used in combination and are selected from one of the following combinations:
[0032] Combination 1: the vulcanizing agent is colloidal sulfur, and the silane coupling agent is a sulfur-containing or sulfur-free silane coupling agent;
[0033] Combination 2: the vulcanizing agent is a thiuram vulcanizing agent, and the silane coupling agent is a sulfur-containing or sulfur-free silane coupling agent;
[0034] Combination three: the vulcanizing agent is a peroxide vulcanizing agent, and the silane coupling agent is a sulfur-free silane coupling agent.
[0035] The molecular structure of silane coupling agent is generally YR-Si(OR)3 (where Y is an organic functional group and SiOR is a silaneoxy group). Silaneoxy group is reactive to inorganic substances, and organic functional groups are reactive or compatible to organic substances. Therefore, when silane coupling agent is between the inorganic and organic interfaces, a bonding layer of organic matrix-silane coupling agent-inorganic matrix can be formed.
[0036] Furthermore, the thiuram vulcanizing agent includes one or more of tetrabenzylthiuram disulfide, bis(40-methylpiperazine)thiuram disulfide, and tetraisobutylthiuram disulfide.
[0037] Furthermore, the peroxide vulcanizing agent includes one or more of diacyl peroxide, tertiary alkyl peroxyester, alkyl hydroperoxide, dialkyl peroxide, and dialkyl peroxyketal.
[0038] Furthermore, the peroxide vulcanizing agent includes one or more of the following: vulcanizing agent DCP (diisopropyl peroxide), vulcanizing agent BPO (benzoyl peroxide), vulcanizing agent BPMC (1,1-di-tert-butylperoxy-3,3,5-trimethylcyclohexane), vulcanizing agent DBPMH (2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane), and vulcanizing agent BIPB (1,3-bis(tert-butylperoxyisopropyl)benzene).
[0039] Further, the sulfur-containing silane coupling agent includes silane coupling agent Si-69 (bis-[γ-(triethoxysilyl)propyl]tetrasulfide); the sulfur-free silane coupling agent includes silane coupling agent A151 (vinyl triethoxysilane), silane coupling agent A171 (vinyl trimethoxysilane), silane coupling agent A172 (vinyl tri(β-methoxyethoxy) silane) or silane coupling agent KH550 (γ-aminopropyl triethoxysilane).
[0040] Furthermore, the zinc oxide is zinc oxide-80 masterbatch.
[0041] The above additives are all raw materials that comply with EU REACH environmental standards.
[0042] Technical solution 2 of the present invention: The preparation method of the green conveyor belt covering rubber comprises the following steps:
[0043] S1, one-stage internal mixing and tamping: first, add the raw rubber into the internal mixer, and mix for 1-3 minutes; then add zinc oxide, stearic acid, antioxidant, and paraffin into the internal mixer, and mix for 1-2 minutes; then add half of the carbon black and white carbon black and all of the silane coupling agent and white carbon black dispersant into the internal mixer, and mix for 1-3 minutes; finally, add the remaining carbon black and white carbon black and cyclohexane oil, mix for 1-3 minutes, and discharge the rubber; tamping the discharged rubber to obtain a first-stage mixed rubber;
[0044] S2, second stage mixing and tamping: the first stage mixed rubber is placed in a mixer for 4-8 hours, an accelerator and a vulcanizing agent are added, mixed for 1-3 minutes, and discharged; the discharged rubber is tamped to obtain a second stage mixed rubber;
[0045] S3. Vulcanization: Let the second-stage mixed rubber stand for 24-72 hours before vulcanization.
[0046] Furthermore, the banburying temperature in the first banburying process is 65-75° C., and the banburying speed is 25-35 rpm.
[0047] Furthermore, the banburying temperature in the second-stage banburying process is 50-70° C., and the banburying speed is 30-35 rpm.
[0048] Furthermore, the specific operation of tamping in step S1 is: adding the discharged rubber material into the open mixer, adjusting the roller distance to 2mm, cutting left and right, passing the roller 6-10 times, and then putting it into the mixer, adjusting the roller distance to 5mm for tamping, one reciprocating back and forth is counted as one time, tamping 6-8 times, and then taking off the sheet and drying the sheet.
[0049] The specific operation of tamping in step S2 is: adding the discharged rubber material into the open mixer, adjusting the roller distance to 2mm, cutting left and right, passing the roller 4-8 times, and then putting it into the mixer, adjusting the roller distance to 5mm for tamping, one reciprocating back and forth is counted as one time, tamping 6-8 times, and then unloading and drying the slices.
[0050] Furthermore, the parking temperature is 23±0.1°C.
[0051] Furthermore, the vulcanization temperature is 145-160° C. and the pressure is 10-20 MPa.
[0052] Furthermore, the vulcanization time is the positive vulcanization time measured by the vulcanization characteristic test of the corresponding two-stage mixed rubber at the corresponding temperature.
[0053] The present invention discloses the following technical effects:
[0054] (1) The present invention adopts a new type of highly dispersed white carbon black plus a white carbon black dispersant and a silane coupling agent to replace most of the carbon black, which effectively reduces the power consumption of the mixed rubber and reduces the mixing temperature. The white carbon black dispersant and the silane coupling agent are used to improve the dispersion of white carbon black in the rubber, thereby ensuring the physical properties of the mixed rubber, effectively reducing the current in the mixing process of the internal mixer, and also reducing the large amount of particulate pollution caused by the scattering of carbon black during the mixing process, reducing the emission of dust and smoke, and achieving energy saving, environmental protection, and carbon reduction in the production process.
[0055] (2) The present invention proposes for the first time the concept, characteristics and production requirements of green conveyor belts. Green conveyor belts refer to energy-saving, environmentally friendly and carbon-reducing conveyor belt products. The entire production process practices the concept of green manufacturing, and the application process advocates green use. Green conveyor belts have low running resistance, excellent weather resistance and better wear resistance. The manufacture of green conveyor belts must meet the following overall requirements: 1) Use environmentally friendly, non-toxic and harmless raw materials that comply with the EU REACH environmental standards; 2) The production process achieves low energy consumption, low noise, low dust and low smoke; 3) The product has the advantages of energy saving, safety and environmental protection.
[0056] (3) The technology of using the new type of highly dispersed white carbon black plus white carbon black dispersant and coupling agent to replace most of the carbon black has been tried in sulfur vulcanization system, sulfur-free vulcanization system (thiuram vulcanizing agent vulcanization system) and peroxide vulcanization system, and achieved good results.
[0057] (4) The present invention also creatively discovered that different vulcanization systems require the use of different silane coupling agents, especially in peroxide vulcanization systems, sulfur-containing silane coupling agents cannot be used, otherwise the aging effect will be affected. DETAILED DESCRIPTION
[0058] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0059] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0060] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0061] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.
[0062] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0063] The room temperature referred to in the following examples and comparative examples specifically refers to 20-25°C.
[0064] The raw materials used in the following examples and comparative examples are all common commercially available products, among which:
[0065] The styrene butadiene rubber (SBR) used was SBR-1500;
[0066] The butadiene rubber used is rare earth butadiene rubber (NdBR), also known as neodymium-based butadiene rubber, which is a high-cis polybutadiene rubber obtained by using butadiene as a monomer and hexane as a solvent. Its ultra-high cis structure content makes the molecular chain have a highly stereoregular structure. It is superior to traditional titanium, cobalt, and nickel-based butadiene rubber in terms of tear strength, heat generation, hysteresis loss, and abrasion. It can produce rubber compounds with excellent physical properties. The product has good fatigue resistance, high resilience, and low friction loss.
[0067] The natural rubber (NR) used is national standard 1# rubber produced in Yunnan Farm Reclamation, Hainan Farm Reclamation or Southeast Asian countries;
[0068] The ethylene propylene rubber used is EPDM4045;
[0069] The white carbon black used is white carbon black 1165MP, the DBP absorption is 165-200ml / 100g, and the CTAB specific surface area is 150-180m 2 / g;
[0070] The white carbon black dispersant used is a mixture of 25 parts of C8-C22 fatty acid (specifically stearic acid), 8 parts of protective wax (specifically paraffin), 5 parts of fatty acid ester (specifically polyethylene glycol fatty acid ester PEG-4000MO), 1.5 parts of antioxidant (specifically antioxidant BHT), 4 parts of calcium carbonate and 2 parts of zinc oxide (all by mass). The specific mixing method is: place the C8-C22 fatty acid in a reactor, stir and heat at 100°C, then add the protective wax and fatty acid ester, continue stirring for 15 minutes after the material is completely melted, add the antioxidant, calcium carbonate and zinc oxide and continue stirring for 15 minutes, cool to room temperature, discharge, and crush to obtain the white carbon black dispersant.
[0071] Example 1
[0072] A green conveyor belt covering rubber comprises the following raw materials, calculated by weight: 100 parts of raw rubber (50 parts of NdBR + 50 parts of NR), 3 parts of zinc oxide-80, 1 part of stearic acid, 1.5 parts of antioxidant 4020, 1 part of paraffin, 20 parts of carbon black N330, 40 parts of white carbon black 1165MP, 7 parts of silane coupling agent Si-69, 3 parts of white carbon black dispersant, 1625 parts of naphthenic oil KN401, 1.5 parts of accelerator DM and 2 parts of vulcanizing agent (colloidal sulfur).
[0073] The preparation process is:
[0074] S1, one stage of internal refining and tamping:
[0075] Set the internal mixer temperature to 70°C and the internal mixer speed to 30 rpm;
[0076] 1) Add all the raw rubber into the internal mixer and mix for 2 minutes;
[0077] 2) Add zinc oxide, stearic acid, antioxidant and paraffin into an internal mixer and mix for 1.5 minutes;
[0078] 3) Add half of the carbon black and white carbon black and all the silane coupling agent and white carbon black dispersant into an internal mixer and mix for 2 minutes; then add the remaining carbon black, white carbon black and cyclohexane oil, mix for 3 minutes, and remove the glue;
[0079] 4) adding the rubber material discharged from step 3) into an open mixing mill, adjusting the roller distance to 2 mm, cutting the left and right sides, passing the rollers 8 times, and then putting it into a tamping mill, adjusting the roller distance to 5 mm for tamping, one reciprocating back and forth is counted as one time, tamping 8 times, and then unrolling and drying the sheet to obtain a section of mixed rubber;
[0080] S2, two-stage internal mixing and tamping:
[0081] 5) placing the rubber mix obtained in step 4) at a temperature of 23±0.1° C. for 6 h, then adding it to an internal mixer, setting the internal mixer temperature to 60° C. and the internal mixer speed to 30 rpm, adding an accelerator and a vulcanizing agent, and mixing for 1.5 min before discharging the rubber;
[0082] 6) adding the rubber material discharged from step 5) into an open mill, adjusting the roller distance to 2 mm, cutting the left and right sides, passing the rollers 8 times, and then putting it into a tamping machine, adjusting the roller distance to 5 mm for tamping, one reciprocating back and forth is counted as one time, tamping 8 times, and then unrolling and drying the sheets to obtain a two-stage mixed rubber;
[0083] 7) The two-stage rubber mix obtained in step 6) is stored at a temperature of 23±0.1°C for 24 hours and then vulcanized. The vulcanization temperature is 150°C, the vulcanization pressure is 10 MPa, and the vulcanization time is the positive vulcanization time measured by the vulcanization characteristic test of the two-stage rubber mix at the corresponding temperature. The performance test is performed after the vulcanized sample is stored at room temperature for 12 hours.
[0084] During the first stage of internal mixing, the maximum current, the maximum temperature of the mixed rubber in the internal mixing chamber, the maximum concentration of particulate matter and the maximum concentration of non-methane total hydrocarbons were monitored, as shown in Table 1.
[0085] Example 2
[0086] A green conveyor belt covering rubber, calculated by weight, comprises the following raw materials: 100 parts of raw rubber (SBR-1500), 5 parts of zinc oxide-80, 1 part of stearic acid, 2 parts of antioxidant 4020, 2 parts of paraffin, 20 parts of carbon black N330, 40 parts of white carbon black 1165MP, 25 parts of naphthenic oil KN4016, 3 parts of white carbon black dispersant, 3 parts of silane coupling agent Si-69, 1.5 parts of accelerator DM and 2 parts of vulcanizing agent (tetrabenzylthiuram disulfide).
[0087] The preparation process is:
[0088] S1, one stage of internal refining and tamping:
[0089] Set the internal mixer temperature to 70°C and the internal mixer speed to 30 rpm;
[0090] 1) Add all the raw rubber into the internal mixer and mix for 2 minutes;
[0091] 2) Add zinc oxide, stearic acid, antioxidant and paraffin into an internal mixer and mix for 1.5 minutes;
[0092] 3) Add half of the carbon black and white carbon black and all the silane coupling agent and white carbon black dispersant into an internal mixer and mix for 2 minutes; then add the remaining carbon black, white carbon black and cyclohexane oil, mix for 3 minutes, and remove the glue;
[0093] 4) adding the rubber material discharged from step 3) into an open mixing mill, adjusting the roller distance to 2 mm, cutting the left and right sides, passing the rollers 8 times, and then putting it into a tamping mill, adjusting the roller distance to 5 mm for tamping, one reciprocating back and forth is counted as one time, tamping 8 times, and then unrolling and drying the sheet to obtain a section of mixed rubber;
[0094] S2, two-stage internal mixing and tamping:
[0095] 5) placing the rubber mix obtained in step 4) at a temperature of 23±0.1° C. for 6 h, then adding it to an internal mixer, setting the internal mixer temperature to 60° C. and the internal mixer speed to 30 rpm, adding an accelerator and a vulcanizing agent, and mixing for 1.5 min before discharging the rubber;
[0096] 6) adding the rubber material discharged from step 5) into an open mill, adjusting the roller distance to 2 mm, cutting the left and right sides, passing the rollers 8 times, and then putting it into a tamping machine, adjusting the roller distance to 5 mm for tamping, one reciprocating back and forth is counted as one time, tamping 8 times, and then unrolling and drying the sheets to obtain a two-stage mixed rubber;
[0097] 7) The two-stage rubber mix obtained in step 6) is stored at a temperature of 23±0.1°C for 24 hours and then vulcanized. The vulcanization temperature is 150°C, the vulcanization pressure is 10 MPa, and the vulcanization time is the positive vulcanization time measured by the vulcanization characteristic test of the two-stage rubber mix at the corresponding temperature. The performance test is performed after the vulcanized sample is stored at room temperature for 12 hours.
[0098] During the first stage of internal mixing, the maximum current, the maximum temperature of the mixed rubber in the internal mixing chamber, the maximum concentration of particulate matter and the maximum concentration of non-methane total hydrocarbons were monitored, as shown in Table 1.
[0099] Example 3
[0100] A green conveyor belt covering rubber, the raw material composition is calculated by weight: 100 parts of raw rubber (EPDM4045), 5 parts of zinc oxide-80, 1 part of stearic acid, 1.5 parts of antioxidant 4020, 1 part of paraffin, 20 parts of carbon black N330, 40 parts of white carbon black 1165MP, 7 parts of silane coupling agent KH550, 5 parts of white carbon black dispersant, 25 parts of cyclohexane oil KN4016, 1.5 parts of cross-linking agent TAIC, and 3 parts of vulcanizing agent (DCP).
[0101] The preparation process is:
[0102] S1, one stage of internal refining and tamping:
[0103] Set the internal mixer temperature to 70°C and the internal mixer speed to 30 rpm;
[0104] 1) Add all the raw rubber into the internal mixer and mix for 2 minutes;
[0105] 2) Add zinc oxide, stearic acid, antioxidant and paraffin into an internal mixer and mix for 1.5 minutes;
[0106] 3) Add half of the carbon black and white carbon black and all the silane coupling agent and white carbon black dispersant into an internal mixer and mix for 2 minutes; then add the remaining carbon black, white carbon black and cyclohexane oil, mix for 3 minutes, and remove the glue;
[0107] 4) adding the rubber material discharged from step 3) into an open mixing mill, adjusting the roller distance to 2 mm, cutting the left and right sides, passing the rollers 8 times, and then putting it into a tamping mill, adjusting the roller distance to 5 mm for tamping, one reciprocating back and forth is counted as one time, tamping 8 times, and then unrolling and drying the sheet to obtain a section of mixed rubber;
[0108] S2, two-stage internal mixing and tamping:
[0109] 5) placing the rubber mix obtained in step 4) at a temperature of 23±0.1° C. for 6 h, then adding it to an internal mixer, setting the internal mixer temperature to 60° C. and the internal mixer speed to 30 rpm, adding an accelerator and a vulcanizing agent, and mixing for 1.5 min before discharging the rubber;
[0110] 6) adding the rubber material discharged from step 5) into an open mill, adjusting the roller distance to 2 mm, cutting the left and right sides, passing the rollers 8 times, and then putting it into a tamping machine, adjusting the roller distance to 5 mm for tamping, one reciprocating back and forth is counted as one time, tamping 8 times, and then unrolling and drying the sheets to obtain a two-stage mixed rubber;
[0111] 7) The two-stage rubber mix obtained in step 6) is stored at a temperature of 23±0.1°C for 24 hours and then vulcanized. The vulcanization temperature is 160°C, the vulcanization pressure is 10 MPa, and the vulcanization time is the positive vulcanization time measured by the vulcanization characteristic test of the two-stage rubber mix at the corresponding temperature. The performance test is performed after the vulcanized sample is stored at room temperature for 12 hours.
[0112] During the first stage of internal mixing, the maximum current, the maximum temperature of the mixed rubber in the internal mixing chamber, the maximum concentration of particulate matter and the maximum concentration of non-methane total hydrocarbons were monitored, as shown in Table 1.
[0113] Comparative Example 1
[0114] A conveyor belt covering rubber, the raw material composition is calculated by weight: 100 parts of raw rubber (50 parts of NdBR + 50 parts of NR), 3 parts of zinc oxide-80, 1 part of stearic acid, 1.5 parts of antioxidant 4020, 1 part of paraffin, 60 parts of carbon black N330, 1625 parts of naphthenic oil KN40, 1.5 parts of accelerator DM, 2 parts of vulcanizing agent (colloidal sulfur). The difference from Example 1 is that the carbon black N330 of the same weight is used to replace the white carbon black 1165MP, and the use of the silane coupling agent and the white carbon black dispersant is omitted.
[0115] The preparation process is:
[0116] S1, one stage of internal refining and tamping:
[0117] Set the internal mixer temperature to 70°C and the internal mixer speed to 30 rpm;
[0118] 1) Add all the raw rubber into the internal mixer and mix for 2 minutes;
[0119] 2) Add zinc oxide, stearic acid, antioxidant and paraffin into an internal mixer and mix for 1.5 minutes;
[0120] 3) Add half of the carbon black into the internal mixer and mix for 2 minutes; then add the remaining carbon black and naphthenic oil, mix for 3 minutes, and remove the glue;
[0121] 4) adding the rubber material discharged from step 3) into an open mixing mill, adjusting the roller distance to 2 mm, cutting the left and right sides, passing the rollers 8 times, and then putting it into a tamping mill, adjusting the roller distance to 5 mm for tamping, one reciprocating back and forth is counted as one time, tamping 8 times, and then unrolling and drying the sheet to obtain a section of mixed rubber;
[0122] S2, two-stage internal mixing and tamping:
[0123] 5) placing the rubber mix obtained in step 4) at a temperature of 23±0.1° C. for 6 h, then adding it to an internal mixer, setting the internal mixer temperature to 60° C. and the internal mixer speed to 30 rpm, adding an accelerator and a vulcanizing agent, and mixing for 1.5 min before discharging the rubber;
[0124] 6) adding the rubber material discharged from step 5) into an open mill, adjusting the roller distance to 2 mm, cutting the left and right sides, passing the rollers 8 times, and then putting it into a tamping machine, adjusting the roller distance to 5 mm for tamping, one reciprocating back and forth is counted as one time, tamping 8 times, and then unrolling and drying the sheets to obtain a two-stage mixed rubber;
[0125] 7) The two-stage rubber mix obtained in step 6) is stored at a temperature of 23±0.1°C for 24 hours and then vulcanized. The vulcanization temperature is 150°C, the vulcanization pressure is 10 MPa, and the vulcanization time is the positive vulcanization time measured by the vulcanization characteristic test of the two-stage rubber mix at the corresponding temperature. The performance test is performed after the vulcanized sample is stored at room temperature for 12 hours.
[0126] During the first stage of internal mixing, the maximum current, the maximum temperature of the mixed rubber in the internal mixing chamber, the maximum concentration of particulate matter and the maximum concentration of non-methane total hydrocarbons were monitored, as shown in Table 1.
[0127] Comparative Example 2
[0128] A conveyor belt covering rubber, the raw material composition is calculated by weight: 100 parts of raw rubber (50 parts of NdBR + 50 parts of NR), 3 parts of zinc oxide-80, 1 part of stearic acid, 1.5 parts of antioxidant 4020, 1 part of paraffin, 60 parts of white carbon black 1165MP, 7 parts of silane coupling agent Si-69, 3 parts of white carbon black dispersant, 1625 parts of naphthenic oil KN40, 1.5 parts of accelerator DM, 2 parts of vulcanizing agent (colloidal sulfur). The difference from Example 1 is that the white carbon black 1165MP of the same weight is used instead of carbon black N330.
[0129] The preparation process is the same as that of Comparative Example 1, except that the carbon black in step 3) is replaced by white carbon black.
[0130] During the first stage of internal mixing, the maximum current, the maximum temperature of the mixed rubber in the internal mixing chamber, the maximum concentration of particulate matter and the maximum concentration of non-methane total hydrocarbons were monitored, as shown in Table 1.
[0131] Comparative Example 3
[0132] A conveyor belt covering rubber, the raw material composition is calculated by weight: 100 parts of raw rubber (SBR-1500), 5 parts of zinc oxide-80, 1 part of stearic acid, 2 parts of antioxidant 4020, 2 parts of paraffin, 60 parts of carbon black N330, 1625 parts of naphthenic oil KN40, 1.5 parts of accelerator DM, 2 parts of vulcanizing agent (tetrabenzylthiuram disulfide). The difference from Example 2 is that the carbon black N330 of the same weight is used instead of the white carbon black 1165MP, and the use of the silane coupling agent and the white carbon black dispersant is omitted.
[0133] The preparation process is the same as that of Comparative Example 1.
[0134] During the first stage of internal mixing, the maximum current, the maximum temperature of the mixed rubber in the internal mixing chamber, the maximum concentration of particulate matter and the maximum concentration of non-methane total hydrocarbons were monitored, as shown in Table 1.
[0135] Comparative Example 4
[0136] A conveyor belt covering rubber, the raw material composition is calculated by weight: 100 parts of raw rubber (EPDM4045), 5 parts of zinc oxide-80, 1 part of stearic acid, 1.5 parts of antioxidant 4020, 1 part of paraffin, 60 parts of carbon black N330, 1625 parts of naphthenic oil KN40, 1.5 parts of auxiliary crosslinking agent TAIC, and 3 parts of vulcanizing agent (DCP). The difference from Example 3 is that the same weight of carbon black N330 is used instead of white carbon black 1165MP, and the use of silane coupling agent and white carbon black dispersant is omitted.
[0137] The preparation process is the same as that of Comparative Example 1.
[0138] During the first stage of internal mixing, the maximum current, the maximum temperature of the mixed rubber in the internal mixing chamber, the maximum concentration of particulate matter and the maximum concentration of non-methane total hydrocarbons were monitored, as shown in Table 1.
[0139] Comparative Example 5
[0140] A conveyor belt covering rubber, the raw material composition is calculated by weight: 100 parts of raw rubber (50 parts of NdBR + 50 parts of NR), 3 parts of zinc oxide-80, 1 part of stearic acid, 1.5 parts of antioxidant 4020, 1 part of paraffin, 20 parts of carbon black N330, 40 parts of white carbon black 1165MP, 1625 parts of naphthenic oil KN40, 1.5 parts of accelerator DM, 2 parts of vulcanizing agent (colloidal sulfur). The only difference from Example 1 is that the use of white carbon black dispersant and silane coupling agent is omitted.
[0141] The preparation process is the same as that of Example 1, except that the addition of white carbon black dispersant and silane coupling agent is omitted in step 3).
[0142] During the first stage of internal mixing, the maximum current, the maximum temperature of the mixed rubber in the internal mixing chamber, the maximum concentration of particulate matter and the maximum concentration of non-methane total hydrocarbons were monitored, as shown in Table 1.
[0143] Comparative Example 6
[0144] The same as Example 1, except that the use of silane coupling agent is omitted.
[0145] During the first stage of internal mixing, the maximum current, the maximum temperature of the mixed rubber in the internal mixing chamber, the maximum concentration of particulate matter and the maximum concentration of non-methane total hydrocarbons were monitored, as shown in Table 1.
[0146] Comparative Example 7
[0147] The same as Example 1, except that the use of white carbon black dispersant is omitted.
[0148] During the first stage of internal mixing, the maximum current, the maximum temperature of the mixed rubber in the internal mixing chamber, the maximum concentration of particulate matter and the maximum concentration of non-methane total hydrocarbons were monitored, as shown in Table 1.
[0149] Comparative Example 8
[0150] Same as Example 3, except that the silane coupling agent KH550 is replaced by an equal mass of silane coupling agent Si-69.
[0151] During the first stage of internal mixing, the maximum current, the maximum temperature of the mixed rubber in the internal mixing chamber, the maximum concentration of particulate matter and the maximum concentration of non-methane total hydrocarbons were monitored, as shown in Table 1.
[0152] Test Case
[0153] The performance test was performed on the samples of each embodiment and comparative example after vulcanization and storage at room temperature for 12 hours. During the vulcanization, a suitable mold was selected according to the size of the sample required for the test.
[0154] Test conditions:
[0155] (1) The wear amount was tested on a roller wear tester (high-speed rail testing instrument) at a temperature of 23℃±0.1℃ according to the wear standard GB / T 9867-2008.
[0156] (2) The tan δ test for characterizing rolling resistance at 60°C was conducted using DMAQ800 (DMAQ800 manufactured by TA Corporation, USA) in the tensile mode, with a scanning temperature range of 0-100°C, a frequency of 10 Hz, and a strain amplitude of 5%.
[0157] (3) The tensile strength and elongation at break were tested according to GB / T 528-2009.
[0158] (4) 150℃×168h aging performance test according to GB / T3512-2014.
[0159] The test results are shown in Table 1:
[0160] Table 1
[0161]
[0162] As shown in Table 1, by comparing Example 1 with Comparative Example 1 and Comparative Example 2, it can be found that Comparative Example 1 is a full carbon black formula, Comparative Example 2 is a full white carbon black formula, and Example 1 is 1 / 3 carbon black plus 2 / 3 white carbon black. From the performance comparison, it can be seen that the full carbon black formula is greater than the formula with a large amount of white carbon black in terms of the maximum current of a first-stage banburying, the highest temperature of a first-stage banburying, the maximum concentration of particulate matter in a first-stage banburying, the maximum concentration of non-methane total hydrocarbons in a first-stage banburying, and the rolling resistance test. Since Comparative Example 2 is a full white carbon black formula, the physical properties are slightly worse. Comparative Example 3 is compared with Example 2. The raw rubber is all SBR. The difference is that Comparative Example 3 is full carbon black, and Example 2 is 1 / 3 carbon black plus 2 / 3 white carbon black + white carbon black dispersant + silane coupling agent system. The performance comparison shows that Example 2 is fully superior. Comparison between Example 4 and Example 3, the raw rubber is EPDM, the difference is that Comparison 4 is all carbon black, and Example 3 is 1 / 3 carbon black plus 2 / 3 white carbon black + white carbon black dispersant + silane coupling agent system, and the performance comparison is also fully superior to Example 3. Comparison between Example 5 and Example 1, the difference is that no white carbon black dispersant + silane coupling agent is used, and the performance comparison is not as good as Example 1, because the white carbon black dispersant and silane coupling agent can increase the dispersion of white carbon black, and the coupling agent can decompose the monomer S at high temperature to participate in crosslinking. Comparison between Example 6 and Example 1, the difference is that no silane coupling agent is used, and the performance comparison is not as good as Example 1. Comparison between Example 7 and Example 1, the difference is that no white carbon black dispersant is used, and the performance comparison is not as good as Example 1. Comparison between Example 8 and Example 3, the difference is that different silane coupling agents are used, and the aging performance of Comparison between Example 8 is far worse than that of Example 3. From the above data, it can be seen that the system of white carbon black + white carbon black dispersant + silane coupling agent can effectively reduce the current, mixing temperature, particle content, and non-methane total hydrocarbon content during the internal mixing production process, while improving the wear resistance of the rubber product and reducing rolling resistance. In addition, the silane coupling agent in the peroxide vulcanization system is not suitable for the use of silane coupling agents containing sulfur elements, because the S element decomposed during the vulcanization process will affect the aging effect of the peroxide vulcanization system.
[0163] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A green conveyor belt covering rubber, characterized in that: The raw materials include the following components by mass: 100 parts of raw rubber; Naphthenic oil 0-30 parts; 20-80 parts of carbon black; 20-80 parts of white carbon black; 3-5 parts of white carbon black dispersant; Silane coupling agent 2-15 parts; 0.3 to 5 parts of accelerator or cross-linking agent; 0.2-3 parts of vulcanizing agent; 1-5 parts of zinc oxide; 1-5 parts of stearic acid; Paraffin 0-5 parts; 1 to 4 parts of antioxidant.
2. The green conveyor belt covering rubber as claimed in claim 1, characterized in that: The raw rubber includes one or more of natural rubber, styrene-butadiene rubber, butadiene rubber, and ethylene-propylene rubber; the antioxidant includes one or more of antioxidant RD, antioxidant D, antioxidant 4020, antioxidant H, antioxidant DPD, antioxidant 264, and antioxidant MB; the accelerator includes one or more of accelerator M, accelerator DM, accelerator NS, accelerator D, accelerator DPG, and accelerator MBTS; the co-crosslinking agent includes co-crosslinking agent TAIC.
3. The green conveyor belt covering rubber as claimed in claim 1, characterized in that: The carbon black includes one or more of N220, N234, N330, N375, N339, N650, and N660.
4. The green conveyor belt covering rubber as claimed in claim 1, characterized in that: The white carbon black is highly dispersed nano white carbon black, with a DBP absorption of 165-200 ml / 100 g and a CTAB specific surface area of 150-180 m 2 / g.
5. The green conveyor belt covering rubber according to claim 1, characterized in that: The raw materials of the white carbon black dispersant include the following components by weight: 20-30 parts of C8-C22 fatty acid, 5-10 parts of protective wax, 3-6 parts of fatty acid ester, 1-2 parts of antioxidant, 2-5 parts of calcium carbonate and 1-3 parts of zinc oxide.
6. The green conveyor belt covering rubber according to claim 1, characterized in that: The vulcanizing agent and the silane coupling agent are used in combination and are selected from one of the following combinations: Combination 1: the vulcanizing agent is colloidal sulfur, and the silane coupling agent is a sulfur-containing or sulfur-free silane coupling agent; Combination 2: the vulcanizing agent is a thiuram vulcanizing agent, and the silane coupling agent is a sulfur-containing or sulfur-free silane coupling agent; Combination three: the vulcanizing agent is a peroxide vulcanizing agent, and the silane coupling agent is a sulfur-free silane coupling agent.
7. The method for preparing the green conveyor belt covering rubber according to any one of claims 1 to 6, characterized in that: The following steps are involved: S1, one-stage internal mixing and tamping: first, add the raw rubber into the internal mixer, and mix for 1-3 minutes; then add zinc oxide, stearic acid, antioxidant, and paraffin into the internal mixer, and mix for 1-2 minutes; then add half of the carbon black and white carbon black and all of the silane coupling agent and white carbon black dispersant into the internal mixer, and mix for 1-3 minutes; finally, add the remaining carbon black and white carbon black and cyclohexane oil, mix for 1-3 minutes, and discharge the rubber; tamping the discharged rubber to obtain a first-stage mixed rubber; S2, second stage mixing and tamping: the first stage mixed rubber is placed in a mixer for 4-8 hours, an accelerator and a vulcanizing agent are added, mixed for 1-3 minutes, and discharged; the discharged rubber is tamped to obtain a second stage mixed rubber; S3. Vulcanization: let the second-stage mixed rubber stand for 24-72 hours before vulcanization.
8. The preparation method according to claim 7, characterized in that: The banburying temperature in the first stage of banburying is 65-75° C., and the banburying speed is 25-35 rpm.
9. The preparation method according to claim 7, characterized in that: The banburying temperature in the second-stage banburying process is 50-70° C., and the banburying speed is 30-35 rpm.
10. The preparation method according to claim 7, characterized in that: The vulcanization temperature is 145-160° C. and the pressure is 10-20 MPa.