Energy-saving and environment-friendly door and window sealing rubber strip and preparation method thereof
By using maleic anhydride modified ethylene propylene ternary rubber and other materials in the sealing rubber strip, the problems of deterioration of elasticity, high energy consumption and heavy pollution in the existing sealing rubber strip materials are solved, and the structural stability of the sealing rubber strips is achieved , flame retardancy and durability are improved, suitable for a wide range of architectural decoration applications.
Patent Information
- Application Number
- CN202411137131.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-08
AI Technical Summary
During the use of existing sealant strip materials, there are problems such as deterioration of elasticity, high energy consumption, heavy pollution, strong migration and great harm to the human body. The durability is poor, resulting in a decrease in sealing performance, affecting the building decoration effect and Living environment.
Maleic anhydride modified ethylene propylene tereum rubber, hydrogenated nitrile rubber, composite carbon black, modified glass fiber, flame retardant, plasticizer, coupling agent, anti-aging agent and chitosan, and other materials are used to reasonably match By ratio and modification, sealing strips with high density, flame retardancy, high and low temperature resistance, excellent mechanical properties, and anti-worms and mildew.
It has achieved the improvement of the structural stability, sealing, flame retardant and aging resistance of the sealing rubber strip, extended the service life, reduced energy consumption and pollution, and is suitable for a wide range of applications and provided better thermal insulation and sound insulation effect. and environmentally friendly performance.
Smart Images

Figure BDA0004999736810000091
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of sealing strips, and in particular to an energy-saving and environmentally friendly door and window sealing strip and a preparation method thereof. Background Art
[0002] Door and window sealing strips are a type of seals mainly used for plastic steel doors and windows, aluminum alloy doors and windows, wooden doors and windows and other architectural decorative doors and windows. The plastic steel door and window sealing strips on the market are generally extruded from PVC, modified PVC, EPDM, elastomer sealing strips, silicone and other materials.
[0003] In the process of making building decorative doors and windows, the investment cost of sealing strips accounts for a relatively small proportion, but its role cannot be ignored. The key to the structure of doors and windows lies in their sealing properties, in which sealing strips play a pivotal role. The materials of sealing strips on the current market are generally modified PVC, rubber, fiber, and fluff. The small molecule plasticizers in the modified PVC are easy to migrate to the surface of the product, causing the elasticity of the sealing strip to deteriorate and the material to harden, thus affecting the sealing performance of doors and windows. Rubber sealing strips have the weaknesses of high energy consumption and heavy pollution in the rubber production process. After being used as sealing strips, some of the small molecule additives in them also have The strong migration leads to defects such as poor elasticity and is very harmful to the human body. At present, the most commonly used rubber is EPDM (ethylene propylene diene monomer rubber) sealing strip. Although EPDM itself has good heat resistance, chemical resistance, water resistance, etc., it is an organic polymer material. During use, it will be affected by the combined effects of external environmental factors (such as light, heat, oxygen and corrosive media, etc.), which will cause the gradual deterioration of physical and mechanical properties until it eventually loses its use value. On the surface, it will manifest as cracking, stickiness, hardening, softening, powdering, discoloration and mold, which will bring great inconvenience to people's normal life and office. Summary of the invention
[0004] The purpose of the present application is to provide an energy-saving and environmentally friendly door and window sealing strip and a preparation method thereof in view of the deficiencies in the current technology. The energy-saving and environmentally friendly door and window sealing strip of the present application has the advantages of simple and convenient preparation, dense and stable sealing strip structure, good sealing, high flame retardancy and resistance to high and low temperatures, excellent aging resistance, excellent mechanical properties, thermal insulation and sound insulation, insect repellent and anti-mildew, energy saving and environmental protection, wide application range, long service life, etc.
[0005] In the first aspect, the present application provides an energy-saving and environmentally friendly door and window sealing strip, which adopts the following technical solution: An energy-saving and environment-friendly door and window sealing strip comprises the following raw materials in parts by mass: 70-75 parts of maleic anhydride modified EPDM rubber, 15-20 parts of hydrogenated nitrile rubber, 4-5 parts of zinc oxide, 0.8-1 part of stearic acid, 50-55 parts of composite carbon black, 8-10 parts of modified glass fiber, 5-7 parts of methylisothiazolinone, 3-4 parts of flame retardant, 10-12 parts of plasticizer, 2-3 parts of coupling agent, 3-4 parts of antioxidant, 6-8 parts of chitosan, 1.0-1.5 parts of sulfur and 1-3 parts of accelerator, wherein the composite carbon black is composed of N550 carbon black and modified white carbon black in a mass ratio of 5:3-4.
[0006] By adopting the above technical scheme, the energy-saving and environmentally friendly door and window sealing strip of the present application has fully utilized the advantages of each component by reasonably selecting the raw materials of each component, and has achieved excellent comprehensive performance. Maleic anhydride modified EPDM rubber and hydrogenated nitrile rubber: These two rubbers have good compatibility, making the structure of the sealing strip more compact and stable, and improving the low temperature resistance. At the same time, they provide basic mechanical properties and elasticity for the sealing strip. Zinc oxide, stearic acid, composite carbon black, modified glass fiber: The addition of these fillers and reinforcing agents can further improve the mechanical properties, wear resistance and aging resistance of the sealing strip. Among them, the composite carbon black is composed of N550 carbon black and modified white carbon black, which can improve the thermal conductivity and electrical conductivity of the sealing strip; the modified glass fiber can improve the strength of the sealing strip and reduce the compression permanent deformation. Methylisothiazolinone, flame retardant, plasticizer, coupling agent, antioxidant: The addition of these additives can make the sealing strip have better flame retardancy, high and low temperature resistance, waterproof and aging resistance. Among them, methylisothiazolinone has a broad-spectrum bactericidal effect, which can effectively prevent the sealing strip from moldy and deteriorating; the flame retardant can form a protective layer, slow down the burning speed, and improve safety; the plasticizer can increase the flexibility and processability of the sealing strip; the coupling agent can improve the interfacial bonding force between the filler and the matrix, and improve the mechanical properties; the anti-aging agent can prevent the sealing strip from aging and prolong the service life. Chitosan, sulfur, and accelerator: The addition of these substances can make the sealing strip have good insect repellent and antifungal properties and vulcanization properties. Among them, chitosan has biodegradability and antibacterial properties, which can reduce the pollution of the sealing strip to the environment; sulfur and accelerator are important components of the vulcanization system, which make the sealing strip have good physical properties and chemical stability. In summary, the energy-saving and environmentally friendly door and window sealing strip of the present application has the advantages of simple and convenient preparation, dense and stable structure of the sealing strip, good sealing, high flame retardancy and high and low temperature resistance, excellent aging resistance, excellent mechanical properties, thermal insulation and sound insulation, insect repellent and antifungal, energy saving and environmental protection through the synergistic effect of each component.
[0007] Preferably, the preparation method of the modified silica is to disperse 5 parts of silica in 40 parts of ethanol by mass to obtain a silica dispersion, then heat the silica dispersion to 75°C and add 0.8 parts of γ-aminopropylmethyldiethoxysilane, then heat the temperature to 130°C and continue stirring the reaction for 24 hours, filter and dry to obtain the modified silica.
[0008] By adopting the above technical scheme and modifying white carbon black with aminosilane coupling agent, the compatibility of white carbon black with maleic anhydride modified EPDM rubber and hydrogenated nitrile rubber can be improved, thereby improving the mechanical properties of the sealing strip, while also inhibiting crystallization and improving low temperature performance and aging resistance.
[0009] Preferably, the preparation method of the maleic anhydride modified EPDM rubber is as follows: according to the mass fraction, the temperature of the internal mixer is raised to 170-180° C., the rotation speed is 70-80 rpm, 20 parts of EPDM rubber are added, and after the EPDM rubber is completely melted, 1.7 parts of maleic anhydride and 0.2 parts of benzoyl peroxide are added to react for 60-90 minutes, and then extruded and granulated by an extruder to obtain the maleic anhydride modified EPDM rubber.
[0010] By adopting the above technical scheme, the preparation method of maleic anhydride modified EPDM rubber is an environmentally friendly and energy-saving method, which is used to improve the heat resistance, aging resistance and mechanical strength of EPDM rubber by introducing maleic anhydride groups. At the same time, the method also has the advantages of mild reaction conditions and simple operation, which is conducive to reducing production costs and improving production efficiency. Maleic anhydride modified EPDM rubber has good compatibility with hydrogenated nitrile rubber, which is conducive to improving the compactness and stability of the sealing strip structure and its low temperature resistance.
[0011] Preferably, the ethylene mass content of the EPDM rubber is 48%, and the mass content of the ENB third monomer is 5%.
[0012] Preferably, the method for preparing the modified glass fiber comprises the following steps: S51, according to the mass fractions, put 0.7 parts of dioctadecyl quaternary ammonium salt and 10 parts of glass fibers with a length of 2-5 mm into a solution consisting of 20 parts of anhydrous ethanol and 3 parts of deionized water, and ultrasonicate at 60° C. for 2.0 h to obtain a mixed solution; S52. Add 0.3 parts of vinyl triethoxysilane to the mixed solution according to the mass fraction, perform ultrasonic treatment for 3 hours, let it stand for 12 hours, and then dry it to obtain modified glass fiber.
[0013] By adopting the above technical scheme, the glass fiber is modified by using dioctadecyl quaternary ammonium salt and vinyl triethoxysilane, so that the compatibility of the glass fiber with maleic anhydride modified EPDM rubber and hydrogenated nitrile rubber is improved, the internal structure network of the sealing strip is optimized, and the large permanent deformation of the sealing strip network under high compression is effectively limited, which can produce a lower hysteresis effect, and can simultaneously improve the strength of the sealing strip and reduce the permanent deformation of compression.
[0014] Preferably, the flame retardant is graphene oxide modified 2-carboxyethyl phenyl hypophosphorous acid, and the preparation method of the graphene oxide modified 2-carboxyethyl phenyl hypophosphorous acid comprises the following steps: S61. Prepare an aqueous suspension by mixing 30 parts of hydrotalcite and 45 parts of water in parts by mass; S62, dispersing 150 parts of 2-carboxyethylphenylphosphorous acid and 10 parts of graphene oxide in a solution consisting of 11 parts of γ-aminopropyltrimethoxysilane, 300 parts of ethanol and 40 parts of water, according to weight parts, to obtain a mixed solution; S63. Slowly add the aqueous suspension to the mixed solution, heat to 43°C, stir at 500 rpm, react for 60 minutes, filter, and vacuum dry at 85°C for 24 hours, grind and sieve to obtain graphene oxide modified 2-carboxyethylphenyl hypophosphorous acid with a particle size of 5-10 μm.
[0015] By adopting the above technical scheme, the prepared graphene oxide modified 2-carboxyethylphenyl hypophosphorous acid can release flame retardant gases such as phosphoric acid during combustion, and these gases can form a protective layer, effectively slowing down the combustion speed and preventing the spread of flames, thereby improving the flame retardant properties of the sealing strip. The 2-carboxyethylphenyl hypophosphorous acid modified by γ-aminopropyltrimethoxysilane and graphene oxide has good compatibility with maleic anhydride modified EPDM rubber and hydrogenated nitrile rubber, which is conducive to improving the dispersibility of 2-carboxyethylphenyl hypophosphorous acid in the sealing strip, thereby improving the flame retardant properties and mechanical properties.
[0016] Preferably, the plasticizer is EPDM rubber grafted with maleic anhydride, wherein the mass content of maleic anhydride is 2%.
[0017] Preferably, the coupling agent is composed of γ-methacryloxypropyltrimethoxysilane, γ-chloropropyltrichlorosilane and vinyltrimethoxysilane in a mass ratio of 4:2:3.
[0018] By adopting the above technical scheme, the coupling agent plays a very important role in the preparation of energy-saving and environmentally friendly door and window sealing strips. It can improve the interfacial compatibility between the filler and the matrix resin and improve the overall performance of the composite material. γ-Methacryloxypropyltrimethoxysilane is a commonly used coupling agent, which can form a chemical bond with the polymer molecular chain, thereby enhancing the bonding force between the filler and the matrix resin. At the same time, it also has a cross-linking effect, which can improve the mechanical properties and heat resistance of the material. γ-Chloropropyltrichlorosilane is also a commonly used coupling agent, which can react with the hydroxyl group on the surface of the filler to form a stable chemical bond. In addition, it also has a catalytic curing effect, which can improve the weather resistance and corrosion resistance of the material. Vinyltrimethoxysilane can react with the hydroxyl group on the surface of the filler to form a stable chemical bond. At the same time, it also has a waterproof and oil-proof effect, which can improve the water resistance and oil resistance of the material. The synergistic effect between the three coupling agents can better improve the interfacial compatibility between the filler and the matrix resin and improve the overall performance of the composite material. At the same time, their respective characteristics can also complement each other, so that the final product has better comprehensive performance.
[0019] Preferably, the accelerator is composed of N-cyclohexyl-2-benzothiazole sulfenamide and tetramethylthiuram disulfide in a mass ratio of 2:3; the antioxidant is composed of antioxidant RD and antioxidant MB in a mass ratio of 3:2.
[0020] In the second aspect, the present application provides a method for preparing an energy-saving and environmentally friendly door and window sealing strip, using the following technical scheme: As a general technical concept, the present application also provides a method for preparing the above-mentioned energy-saving and environmentally friendly door and window sealing strip, comprising the following steps: S101. Add maleic anhydride modified EPDM rubber and hydrogenated nitrile rubber to a rubber mixing device according to their weight fractions, stir evenly, then add zinc oxide, stearic acid, composite carbon black, modified glass fiber, coupling agent, methylisothiazolinone, flame retardant and chitosan for mixing, then add plasticizer, antioxidant and accelerator, mix evenly and add sulfur to obtain a mixed rubber; S102, heating and pressurizing the rubber mixture for vulcanization reaction, wherein the temperature for vulcanization is 170-180°C and the vulcanization pressure is 180-200kg / cm 2 The vulcanization time is 10-14 minutes, and finally it is extruded by an extruder to form energy-saving and environmentally friendly door and window sealing strips.
[0021] By adopting the above technical scheme, the preparation method of the energy-saving and environmentally friendly door and window sealing strip of the present application is simple, the operation and control are convenient, the product quality is high, the cost is low, and it is conducive to industrial production.
[0022] In summary, the beneficial technical effects of this application are: 1. Easy preparation: By optimizing the formula and process, the preparation process is simplified and the production efficiency is improved.
[0023] 2. Stable structure: The use of raw materials such as maleic anhydride modified EPDM rubber makes the structure of the sealing strip more compact and stable, effectively preventing the penetration of gas and moisture.
[0024] 3. Good sealing: The sealing between the rubber strips and doors and windows is significantly improved, which effectively prevents the transfer of heat and noise and improves the overall performance of doors and windows.
[0025] 4. High flame retardancy: The addition of graphene oxide modified 2-carboxyethylphenyl hypophosphorous acid allows the release of flame-flammable gases such as phosphoric acid during the combustion process to form a protective layer, which effectively slows down the combustion speed and improves the flame retardant properties.
[0026] 5. Good low temperature resistance: By selecting raw materials with excellent high and low temperature resistance and reasonable ratio design, the sealing strip can maintain stable performance under extreme temperature conditions.
[0027] 6. Excellent aging resistance: The use of raw materials such as composite carbon black enhances the waterproofness and aging resistance of the rubber strip and extends its service life.
[0028] 7. Excellent mechanical properties: Through the synergistic effect of additives such as coupling agents and antioxidants, the mechanical properties of the rubber strip are improved, enabling it to withstand greater stress and deformation.
[0029] 8. Good thermal insulation and sound insulation effects: The airtightness of the sealing strip ensures good thermal insulation and sound insulation effects, providing people with a more comfortable living environment.
[0030] 9. Insect repellent and anti-fungal: The addition of natural materials such as chitosan has a certain insect repellent and anti-fungal effect, which helps to keep the indoor environment clean and hygienic.
[0031] 10. Energy saving and environmental protection: The entire production process has no pollution emissions, which is in line with the concept of green environmental protection; at the same time, the sealing strip can effectively reduce energy consumption during use and achieve energy saving and emission reduction. DETAILED DESCRIPTION
[0032] The embodiments of the present application will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. In the examples, if specific conditions are not specified, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0033] In the following preparation examples and embodiments, 1 part means 1 kg.
[0034] Preparation Example 1 Preparation of modified white carbon black The preparation method of modified silica is as follows: 5 parts of silica are dispersed in 40 parts of ethanol according to the mass fraction to obtain a silica dispersion, and then the silica dispersion is heated to 75°C and 0.8 parts of γ-aminopropylmethyldiethoxysilane are added, and then the temperature is raised to 130°C and the reaction is continuously stirred for 24 hours, filtered, and dried to obtain modified silica.
[0035] Preparation Example 2 Preparation of maleic anhydride modified EPDM rubber The preparation method of maleic anhydride modified EPDM rubber is as follows: according to the mass fraction, the temperature of an internal mixer is raised to 178° C. and the rotation speed is 77 rpm, 20 parts of EPDM rubber are added, and after the EPDM rubber is completely melted, 1.7 parts of maleic anhydride and 0.2 parts of benzoyl peroxide are added to react for 80 minutes, and then extruded and granulated by an extruder to obtain the maleic anhydride modified EPDM rubber, wherein the ethylene mass content of the EPDM rubber is 48%, and the mass content of the ENB third monomer is 5%.
[0036] Preparation Example 3 Preparation of modified glass fiber The preparation method of the modified glass fiber comprises the following steps: S51, according to the mass fractions, put 0.7 parts of dioctadecyl quaternary ammonium salt and 10 parts of glass fibers with a length of 2-5 mm into a solution consisting of 20 parts of anhydrous ethanol and 3 parts of deionized water, and ultrasonicate at 60° C. for 2.0 h to obtain a mixed solution; S52. Add 0.3 parts of vinyl triethoxysilane to the mixed solution according to the mass fraction, perform ultrasonic treatment for 3 hours, let it stand for 12 hours, and then dry it to obtain modified glass fiber.
[0037] Preparation Example 4 Preparation of Graphene Oxide Modified 2-Carboxyethylphenyl Hypophosphorous Acid The preparation method of graphene oxide modified 2-carboxyethylphenyl hypophosphorous acid comprises the following steps: S61. Prepare an aqueous suspension by mixing 30 parts of hydrotalcite and 45 parts of water in parts by mass; S62, dispersing 150 parts of 2-carboxyethylphenylphosphorous acid and 10 parts of graphene oxide in a solution consisting of 11 parts of γ-aminopropyltrimethoxysilane, 300 parts of ethanol and 40 parts of water, according to weight parts, to obtain a mixed solution; S63. Slowly add the aqueous suspension to the mixed solution, heat to 43°C, stir at 500 rpm, react for 60 minutes, filter, and vacuum dry at 85°C for 24 hours, grind and sieve to obtain graphene oxide modified 2-carboxyethylphenyl hypophosphorous acid with a particle size of 5-10 μm.
[0038] Example 1 An energy-saving and environmentally friendly door and window sealing strip, comprising the following raw materials in parts by weight: 70 parts of maleic anhydride modified EPDM rubber, 15 parts of hydrogenated nitrile rubber, 4 parts of zinc oxide, 0.8 parts of stearic acid, 50 parts of composite carbon black, 8 parts of modified glass fiber, 5 parts of methylisothiazolinone, 3 parts of flame retardant, 10 parts of plasticizer, 2 parts of coupling agent, 3 parts of antioxidant, 6 parts of chitosan, 1.0 part of sulfur, and 1 part of accelerator, wherein the composite carbon black is composed of N550 carbon black and modified white carbon black in a mass ratio of 5:4, the flame retardant is oxidized Graphene modified 2-carboxyethylphenyl hypophosphorous acid, the plasticizer is ethylene propylene rubber grafted maleic anhydride, wherein the mass content of maleic anhydride is 2%, the coupling agent is composed of γ-methacryloxypropyltrimethoxysilane, γ-chloropropyltrichlorosilane and vinyltrimethoxysilane in a mass ratio of 4:2:3, the accelerator is composed of N-cyclohexyl-2-benzothiazole sulfonamide and tetramethylthiuram disulfide in a mass ratio of 2:3; the antioxidant is composed of antioxidant RD and antioxidant MB in a mass ratio of 3:2.
[0039] The above-mentioned method for preparing an energy-saving and environmentally friendly door and window sealing strip comprises the following steps: S101. Add maleic anhydride modified EPDM rubber and hydrogenated nitrile rubber to a rubber mixing device according to their weight fractions, stir evenly, then add zinc oxide, stearic acid, composite carbon black, modified glass fiber, coupling agent, methylisothiazolinone, flame retardant and chitosan for mixing, then add plasticizer, antioxidant and accelerator, mix evenly and add sulfur to obtain a mixed rubber; S102, heating and pressurizing the rubber mix for vulcanization reaction, wherein the temperature for vulcanization is 170°C and the vulcanization pressure is 200kg / cm 2 The vulcanization time is 14 minutes, and finally it is extruded by an extruder to form energy-saving and environmentally friendly door and window sealing strips.
[0040] Example 2 An energy-saving and environmentally friendly door and window sealing strip, comprising the following raw materials in parts by weight: 75 parts of maleic anhydride modified EPDM rubber, 20 parts of hydrogenated nitrile rubber, 5 parts of zinc oxide, 1 part of stearic acid, 55 parts of composite carbon black, 10 parts of modified glass fiber, 7 parts of methylisothiazolinone, 4 parts of flame retardant, 12 parts of plasticizer, 3 parts of coupling agent, 4 parts of antioxidant, 8 parts of chitosan, 1.5 parts of sulfur, and 3 parts of accelerator, wherein the composite carbon black is composed of N550 carbon black and modified white carbon black in a mass ratio of 5:3, and the flame retardant is silica oxide. Graphene modified 2-carboxyethylphenyl hypophosphorous acid, the plasticizer is ethylene propylene rubber grafted maleic anhydride, wherein the mass content of maleic anhydride is 2%, the coupling agent is composed of γ-methacryloxypropyltrimethoxysilane, γ-chloropropyltrichlorosilane and vinyltrimethoxysilane in a mass ratio of 4:2:3, the accelerator is composed of N-cyclohexyl-2-benzothiazole sulfonamide and tetramethylthiuram disulfide in a mass ratio of 2:3; the antioxidant is composed of antioxidant RD and antioxidant MB in a mass ratio of 3:2.
[0041] The above-mentioned method for preparing an energy-saving and environmentally friendly door and window sealing strip comprises the following steps: S101. Add maleic anhydride modified EPDM rubber and hydrogenated nitrile rubber to a rubber mixing device according to their weight fractions, stir evenly, then add zinc oxide, stearic acid, composite carbon black, modified glass fiber, coupling agent, methylisothiazolinone, flame retardant and chitosan for mixing, then add plasticizer, antioxidant and accelerator, mix evenly and add sulfur to obtain a mixed rubber; S102, heating and pressurizing the rubber mix for vulcanization reaction, wherein the temperature for vulcanization is 180°C and the vulcanization pressure is 180kg / cm 2 The vulcanization time is 10 minutes, and finally it is extruded by an extruder to form energy-saving and environmentally friendly door and window sealing strips.
[0042] Example 3 An energy-saving and environmentally friendly door and window sealing strip, comprising the following raw materials in parts by weight: 73 parts of maleic anhydride modified EPDM rubber, 18 parts of hydrogenated nitrile rubber, 4.5 parts of zinc oxide, 0.9 parts of stearic acid, 53 parts of composite carbon black, 9 parts of modified glass fiber, 6 parts of methylisothiazolinone, 3.6 parts of flame retardant, 11 parts of plasticizer, 2.5 parts of coupling agent, 3.6 parts of antioxidant, 7 parts of chitosan, 1.3 parts of sulfur, and 2 parts of accelerator, wherein the composite carbon black is composed of N550 carbon black and modified white carbon black in a mass ratio of 5:3.5, and the flame retardant is 1.3 parts of accelerator. The igniter is graphene oxide modified 2-carboxyethylphenylphosphorous acid, the plasticizer is ethylene propylene rubber grafted maleic anhydride, wherein the mass content of maleic anhydride is 2%, the coupling agent is composed of γ-methacryloxypropyltrimethoxysilane, γ-chloropropyltrichlorosilane and vinyltrimethoxysilane in a mass ratio of 4:2:3, the accelerator is N-cyclohexyl-2-benzothiazolesulfonamide and tetramethylthiuram disulfide in a mass ratio of 2:3; the antioxidant is composed of antioxidant RD and antioxidant MB in a mass ratio of 3:2.
[0043] The above-mentioned method for preparing an energy-saving and environmentally friendly door and window sealing strip comprises the following steps: S101. Add maleic anhydride modified EPDM rubber and hydrogenated nitrile rubber to a rubber mixing device according to their weight fractions, stir evenly, then add zinc oxide, stearic acid, composite carbon black, modified glass fiber, coupling agent, methylisothiazolinone, flame retardant and chitosan for mixing, then add plasticizer, antioxidant and accelerator, mix evenly and add sulfur to obtain a mixed rubber; S102, heating and pressurizing the rubber mix for vulcanization reaction, wherein the temperature for vulcanization is 176°C and the vulcanization pressure is 190kg / cm 2 The vulcanization time is 12 minutes, and finally it is extruded by an extruder to form energy-saving and environmentally friendly door and window sealing strips.
[0044] Comparative Example 1 The same as Example 3, except that an equal amount of EPDM rubber (the ethylene mass content of the EPDM rubber is 48%, and the mass content of the ENB third monomer is 5%) is used to replace the maleic anhydride modified EPDM rubber.
[0045] Comparative Example 2 The same as Example 3, except that an equal amount of 2-carboxyethylphenyl hypophosphorous acid is used instead of graphene oxide-modified 2-carboxyethylphenyl hypophosphorous acid.
[0046] Comparative Example 3 The same as Example 3, except that an equal amount of white carbon black is used instead of modified white carbon black.
[0047] Comparative Example 4 The same as Example 3, except that an equal amount of glass fibers with a length of 2-5 mm are used instead of the modified glass fibers.
[0048] Comparative Example 5 The same as Example 3, except that the coupling agent is γ-methacryloxypropyltrimethoxysilane.
[0049] Comparative Example 6 The same as Example 3, except that the coupling agent is γ-chloropropyltrichlorosilane.
[0050] Comparative Example 7 The same as Example 3, except that the coupling agent is vinyltrimethoxysilane.
[0051] Performance Testing The energy-saving and environmentally friendly door and window sealing strips prepared in Examples 1 to 3 and Comparative Examples 1 to 7 were subjected to performance tests, and the results are shown in Table 1.
[0052] Tensile strength and elongation at break: refer to GB / T 528-2009 Determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber to test tensile strength and elongation, and the tensile rate is 500mm / min; Flame retardant test: refer to the test method in ANSI / UL-94-1985, vertical burning test according to 94V-0, 94V-1, 94V-2, the test strip thickness is 1mm; Brittle temperature: tested according to ASTM D-746 standard; Aging resistance: According to GB / T 3512-2014 "Hot air accelerated aging and heat resistance test for vulcanized rubber or thermoplastic rubber", the temperature is 180℃ and the aging time is 48h; Compression set: Test compression set according to GB / T7759-1996 A method, test conditions: 100℃x168h, 25% compression rate A method; The antibacterial property is tested according to the QB / T2591-2003 standard. The antibacterial judgment standard is: the antibacterial rate is greater than or equal to 99% for level I, which is called strong antibacterial effect; the antibacterial rate is greater than or equal to 90% for level II, which is called antibacterial effect; the antibacterial rate is less than 90% for no antibacterial effect.
[0053] The criteria for judging mildew resistance are as follows: Level 0 means no growth, i.e. no mold growth is observed under a microscope (magnification 50 times); Level 1 means trace growth, i.e. growth is visible to the naked eye, but the growth coverage area does not exceed 10%; Level 2 means the growth area exceeds 10%.
[0054] Table 1 Performance test Analyzing the data in Table 1, we can see that: 1) The energy-saving and environmentally friendly door and window sealing strips prepared in Examples 1 to 3 have the advantages of simple and convenient preparation, dense and stable sealing strip structure, good sealing, high flame retardancy and good low temperature resistance, excellent aging resistance, excellent mechanical properties, insect repellent and anti-mildew, energy saving and environmental protection, wide application range, long service life, etc.
[0055] 2) The performance comparison analysis of the energy-saving and environmentally friendly door and window sealing strips prepared in Example 3 and Comparative Example 1 shows that the use of maleic anhydride-modified EPDM rubber improves the heat resistance, aging resistance and mechanical strength of the EPDM rubber by introducing maleic anhydride groups. At the same time, maleic anhydride-modified EPDM rubber has good compatibility with hydrogenated nitrile rubber, which is conducive to improving the compactness and stability of the structure and low temperature resistance of the sealing strip, thereby improving the overall performance of the sealing strip.
[0056] 3) The performance comparison analysis of the energy-saving and environmentally friendly door and window sealing strips prepared in combination with Example 3 and Comparative Example 2 shows that the prepared graphene oxide modified 2-carboxyethylphenyl hypophosphorous acid can release flame retardant gases such as phosphoric acid during combustion, and these gases can form a protective layer, effectively slowing down the combustion speed and preventing the spread of flames, thereby improving the flame retardant properties of the sealing strip. The 2-carboxyethylphenyl hypophosphorous acid modified by γ-aminopropyltrimethoxysilane and graphene oxide has good compatibility with maleic anhydride modified ethylene propylene rubber and hydrogenated nitrile rubber, which is beneficial to improve the dispersibility of 2-carboxyethylphenyl hypophosphorous acid in the sealing strip, thereby improving the flame retardant properties and mechanical properties.
[0057] 4) The comparative analysis of the performance of the energy-saving and environmentally friendly door and window sealing strips prepared in Example 3 and Comparative Example 3 shows that the modification of white carbon black with an aminosilane coupling agent can improve the compatibility of white carbon black with maleic anhydride-modified EPDM rubber and hydrogenated nitrile rubber, thereby improving the mechanical properties of the sealing strip, while also inhibiting crystallization and improving low temperature performance and aging resistance.
[0058] 5) The performance comparison analysis of the energy-saving and environmentally friendly door and window sealing strips prepared in Example 3 and Comparative Example 4 shows that the modification of glass fiber by disoctadecyl quaternary ammonium salt and vinyl triethoxysilane improves the compatibility of glass fiber with maleic anhydride-modified EPDM rubber and hydrogenated nitrile rubber, optimizes the internal structure network of the sealing strip, effectively limits the large permanent deformation of the sealing strip network under high compression, can produce a lower hysteresis, and can simultaneously improve the strength of the sealing strip and reduce the compression permanent deformation.
[0059] 6) The performance comparison analysis of the energy-saving and environmentally friendly door and window sealing strips prepared in Example 3 and Comparative Example 5 and Comparative Example 7 shows that the coupling agent is composed of γ-methacryloxypropyltrimethoxysilane, γ-chloropropyltrichlorosilane and vinyltrimethoxysilane in a mass ratio of 4:2:3. By utilizing the synergistic effect between them, the interfacial compatibility between the filler and the matrix resin can be better improved, and the overall performance of the composite material can be improved. At the same time, their respective characteristics can also complement each other, so that the final product has better comprehensive performance.
[0060] The above embodiments are only used to explain the technical solutions of the present application rather than to limit them. Although the above embodiments provide a specific description of the present application, relevant technical personnel should understand that the specific implementation modes of the present invention can still be modified or replaced by equivalents, and any modifications and equivalent replacements that do not depart from the spirit and scope of the present application should be included in the scope of protection of the present application.
Claims
1. An energy-saving and environmentally friendly door and window sealing strip, characterized in that: The invention comprises the following raw materials in parts by weight: 70-75 parts of maleic anhydride modified EPDM rubber, 15-20 parts of hydrogenated nitrile rubber, 4-5 parts of zinc oxide, 0.8-1 parts of stearic acid, 50-55 parts of composite carbon black, 8-10 parts of modified glass fiber, 5-7 parts of methylisothiazolinone, 3-4 parts of flame retardant, 10-12 parts of plasticizer, 2-3 parts of coupling agent, 3-4 parts of antioxidant, 6-8 parts of chitosan, 1.0-1.5 parts of sulfur and 1-3 parts of accelerator, wherein the composite carbon black is composed of N550 carbon black and modified white carbon black in a mass ratio of 5:3-4.
2. The energy-saving and environmentally friendly door and window sealing strip according to claim 1, characterized in that: The preparation method of the modified silica is as follows: 5 parts of silica are dispersed in 40 parts of ethanol according to the mass fraction to obtain a silica dispersion, the silica dispersion is heated to 75° C., 0.8 parts of γ-aminopropylmethyldiethoxysilane is added, the temperature is then raised to 130° C., the reaction is continued with stirring for 24 hours, filtering and drying to obtain the modified silica.
3. The energy-saving and environmentally friendly door and window sealing strip according to claim 1, characterized in that: The preparation method of the maleic anhydride modified EPDM rubber is as follows: according to the mass fraction, the temperature of an internal mixer is raised to 170-180° C., the rotation speed is 70-80 rpm, 20 parts of EPDM rubber are added, and after the EPDM rubber is completely melted, 1.7 parts of maleic anhydride and 0.2 parts of benzoyl peroxide are added to react for 60-90 minutes, and then extruded and granulated by an extruder to obtain the maleic anhydride modified EPDM rubber.
4. The energy-saving and environmentally friendly door and window sealing strip according to claim 3, characterized in that: The ethylene mass content of the EPDM rubber is 48%, and the mass content of the ENB third monomer is 5%.
5. The energy-saving and environmentally friendly door and window sealing strip according to claim 1, characterized in that: The preparation method of the modified glass fiber comprises the following steps: S51, according to the mass fractions, put 0.7 parts of dioctadecyl quaternary ammonium salt and 10 parts of glass fibers with a length of 2-5 mm into a solution consisting of 20 parts of anhydrous ethanol and 3 parts of deionized water, and ultrasonicate at 60° C. for 2.0 h to obtain a mixed solution; S52. Add 0.3 parts of vinyl triethoxysilane to the mixed solution according to the mass fraction, perform ultrasonic treatment for 3 hours, let it stand for 12 hours, and then dry it to obtain modified glass fiber.
6. The energy-saving and environmentally friendly door and window sealing strip according to claim 1, characterized in that: The flame retardant is graphene oxide modified 2-carboxyethyl phenyl hypophosphorous acid, and the preparation method of the graphene oxide modified 2-carboxyethyl phenyl hypophosphorous acid comprises the following steps: S61. Prepare an aqueous suspension by mixing 30 parts of hydrotalcite and 45 parts of water in parts by mass; S62, dispersing 150 parts of 2-carboxyethylphenylphosphorous acid and 10 parts of graphene oxide in a solution consisting of 11 parts of γ-aminopropyltrimethoxysilane, 300 parts of ethanol and 40 parts of water, according to weight parts, to obtain a mixed solution; S63. Slowly add the aqueous suspension to the mixed solution, heat to 43°C, stir at 500 rpm, react for 60 minutes, filter, and vacuum dry at 85°C for 24 hours, grind and sieve to obtain graphene oxide modified 2-carboxyethylphenyl hypophosphorous acid with a particle size of 5-10 μm.
7. The energy-saving and environmentally friendly door and window sealing strip according to claim 1, characterized in that: The plasticizer is EPDM rubber grafted with maleic anhydride, wherein the mass content of maleic anhydride is 2%.
8. The energy-saving and environmentally friendly door and window sealing strip according to claim 1, characterized in that: The coupling agent is composed of γ-methacryloxypropyltrimethoxysilane, γ-chloropropyltrichlorosilane and vinyltrimethoxysilane in a mass ratio of 4:2:
3.
9. The energy-saving and environmentally friendly door and window sealing strip according to claim 1, characterized in that: The accelerator is composed of N-cyclohexyl-2-benzothiazole sulfenamide and tetramethylthiuram disulfide in a mass ratio of 2:3; the antioxidant is composed of antioxidant RD and antioxidant MB in a mass ratio of 3:
2.
10. A method for preparing an energy-saving and environmentally friendly door and window sealing strip according to any one of claims 1 to 9, characterized in that: The following steps are involved: S101. Add maleic anhydride modified EPDM rubber and hydrogenated nitrile rubber to a rubber mixing device according to their weight fractions, stir evenly, then add zinc oxide, stearic acid, composite carbon black, modified glass fiber, coupling agent, methylisothiazolinone, flame retardant and chitosan for mixing, then add plasticizer, antioxidant and accelerator, mix evenly and add sulfur to obtain a mixed rubber; S102, heating and pressurizing the rubber mix for vulcanization reaction, wherein the temperature for vulcanization is 170-180°C and the vulcanization pressure is 180-200kg / cm 2 The vulcanization time is 10-14 minutes, and finally it is extruded by an extruder to form energy-saving and environmentally friendly door and window sealing strips.
Citation Information
Cited By
Dense hole-forming sealing rubber strip and preparation method thereof
CN120484390A