High-thermal-conductivity epoxy molding compound for packaging high-power device and preparation method of high-thermal-conductivity epoxy molding compound
By using modified spherical aluminum nitride as thermal conductivity filler in epoxy plastic seals, the problem of insufficient thermal conductivity in the prior art is solved, the high thermal conductivity requirements of high-power devices are achieved, and production costs and equipment wear are reduced.
Patent Information
- Application Number
- CN202411104736.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-08
AI Technical Summary
Existing polymer packaging materials lack thermal conductivity in high-power chips, resulting in untimely heat dissipation, affecting product reliability. Commonly used thermal fillers such as angular crystalline silicon powder wear out the equipment and have poor processing performance under high filler volume. , the thermal conductivity can only be increased to 2-4W/m·K, and cannot meet the thermal conductivity requirements of high-power devices.
Modified spherical aluminum nitride of different particle sizes is used as thermal conductivity filler, and the thermal conductivity filler with high intrinsic thermal conductivity is formed through spray equipment, and the ratio is optimized in epoxy plastic sealing material, and high thermal conductivity is prepared in combination with the twin screw extrusion mechanism. The amount of thermally conductive filler can reach 70%~94%.
The thermal conductivity of epoxy plastic sealing materials reaches 6W/m·K and above, reducing equipment wear, improving electrical performance and reliability, meeting the thermal conductivity requirements of high-power devices, and reducing production costs.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of semiconductor devices, and in particular to an epoxy molding compound with high thermal conductivity for packaging high-power devices and a preparation method thereof. Background Art
[0002] Epoxy molding compound is an electronic packaging material, mainly used for packaging and protection of semiconductor chips. Epoxy molding compound has become one of the most common packaging materials due to its low cost, high reliability and high packaging efficiency. However, with the continuous development of science and technology, the integration of chip functions, high power and miniaturization of chip packaging have put forward higher requirements on the performance of packaging materials. As the power of the chip increases and the heat generation increases, the heat generated also increases. If the heat is not dissipated in time, it is very easy to cause the chip to be damaged, resulting in a decrease in product reliability.
[0003] At present, thermal conductive interface materials are generally prepared from polymer composite thermal conductive fillers, and the most mainstream theory of its thermal conductivity mechanism is the thermal conductivity path theory. Generally speaking, there are no free electrons in most polymers, molecular motion is difficult, and heat conduction mainly depends on lattice vibration, but most of the polymers are amorphous parts, which greatly limits the heat conduction inside the molecules. Filled thermal conductive polymer composite materials fill the shortcomings of low thermal conduction efficiency inside polymers due to the addition of fillers with high thermal conductivity. The improvement of the thermal conductivity of filled thermal conductive composite materials mainly depends on the addition of high thermal conductivity fillers to low thermal conductivity resins. According to the thermal conductivity path theory, when the amount of fillers is reduced, although the fillers can be evenly dispersed in the resin, the filler particles are still the resin matrix with poor thermal conductivity, and a good thermal conductivity path cannot be formed between the fillers, which does not improve the thermal conductivity of the composite material much; once the amount of thermal conductive fillers added exceeds the critical value, the fillers contact each other in the resin matrix to form an internal thermal conductivity path, and the thermal conductivity of the composite material will increase rapidly. At the same time, if only spherical thermal conductive fillers of the same particle size are used, there will still be a large number of gaps between the spheres occupied by the resin matrix with low thermal conductivity, and the thermal conductivity of the composite material cannot be further improved. Therefore, the use of two or more thermal conductive fillers of different particle sizes in combination becomes the best choice to improve the thermal conductivity of the composite material.
[0004] In the prior art, angular crystalline silicon powder or spherical alumina is mostly used as thermal conductive filler, and the purpose of improving the thermal conductivity is achieved by continuously increasing the filler amount or selecting fillers with different geometric characteristics. However, on the one hand, the angular crystalline silicon powder has many edges and corners and high hardness, which causes great wear to the mixing equipment. The iron impurities in the equipment are introduced into the plastic packaging material, which has an adverse effect on the electrical insulation performance. At the same time, a high filler amount is bound to have an adverse effect on the processing performance and packaging performance of the plastic packaging material. A high filler amount will cause its viscosity to increase, the fluidity to deteriorate, and even cause impact on the gold wire on the surface of the chip, causing it to break. On the other hand, even if the filler amount of angular crystalline silicon powder or spherical alumina is increased to 88%~92% as a thermal conductive filler, its thermal conductivity can only be increased to 2~4W / m·K, which is still insufficient to meet the thermal conductivity requirements of current high-power devices. Summary of the invention
[0005] The present invention aims to solve at least one of the technical problems existing in the related art. To this end, the first object of the present invention is to provide an epoxy molding compound with high thermal conductivity for packaging high-power devices; the second object of the present invention is to provide a method for preparing the epoxy molding compound with high thermal conductivity for packaging high-power devices.
[0006] In order to achieve the first purpose, the technical solution adopted by the present invention is: A high thermal conductivity epoxy molding compound for packaging high power devices, the composition and mass percentage of each component are as follows: Epoxy resin, 3%~15%; Curing agent, 1.5%~10%; Thermal conductive filler, 70%~94%; Curing accelerator, 0.05%~3%; Release agent, 0.05%~2%; Stress release agent, 0.02%~1%; Silane coupling agent, 0.1%~3%; Colorant, 0.02%~1%; Flame retardant, 0.05%~3%; Ion capture agent, 0.05%~3%; Wherein, the thermal conductive filler is composed of modified spherical aluminum nitride with different particle sizes.
[0007] Furthermore, the particle size of the spherical aluminum nitride ranges from 0.5 μm to 40 μm.
[0008] Furthermore, the epoxy resin is at least one of o-cresol epoxy resin, cyclopentadiene epoxy resin and aromatic epoxy resin.
[0009] Furthermore, the curing agent is a phenolic resin curing agent; the curing agent accelerator is at least one of an imidazole accelerator, an organic phosphorus accelerator and its derivative accelerator, and a bicyclic amidine accelerator and its derivative accelerator.
[0010] Furthermore, the release agent is at least one of carnauba wax, montan wax and oxidized polyethylene wax.
[0011] Furthermore, the stress release agent is at least one of epoxidized silicone oil and epoxidized polybutadiene.
[0012] Furthermore, the silane coupling agent is at least one of 3-aminopropyltriethoxysilane, 3-glycidoxypropyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane, N-phenyl-3-aminopropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane.
[0013] Further, the flame retardant is at least one of aluminum hydroxide, zinc borate, melamine cyanurate and organophosphorus flame retardant; The ion capture agent is hydrotalcite.
[0014] In order to achieve the second purpose, the technical solution adopted by the present invention is: A method for preparing a high thermal conductivity epoxy molding compound for packaging high power devices, which is used to prepare the high thermal conductivity epoxy molding compound for packaging high power devices as described in any one of the above, comprising the following steps: S100, weighing a curing agent, a curing accelerator, a flame retardant, a release agent, and an ion capture agent according to the composition and the mass percentage of each component, and dispersing the weighed components for 1 h to 2 h to obtain a mixture I; S200, uniformly mixing the modified spherical aluminum nitride filler, the silane coupling agent, the stress release agent and the colorant to obtain a mixture II; S300, uniformly mixing mixture I, mixture II and epoxy resin to obtain an epoxy molding compound mixture; S400, extruding the epoxy molding compound mixture through a 50° C. to 100° C. twin-screw extruder to obtain a high thermal conductivity epoxy molding compound.
[0015] Further, in step S200, the modified spherical aluminum nitride thermally conductive filler is prepared by the following steps: S201, adding spherical aluminum nitride to a high-speed mixing pot, stirring and heating to 20°C to 40°C, adding deionized water to the high-speed mixing pot in batches using a spray device, collecting and testing ammonia generated by hydrolysis using a negative pressure device, and stopping adding deionized water when the hydrolysis rate of the spherical aluminum nitride is within the range of 1% to 10%; S202, adding tetraethyl orthosilicate into a high-speed mixing pot by using a spray device, the added amount being 0.2% to 5% by mass of the spherical aluminum nitride, and coating the aluminum nitride with tetraethyl orthosilicate to obtain a modified spherical aluminum nitride filler.
[0016] The above one or more technical solutions in the embodiments of the present invention have at least one of the following technical effects: The invention provides a high thermal conductivity epoxy molding compound for packaging high-power devices. In the formula composition, modified spherical aluminum nitride is used as a thermal conductive filler. The thermal conductive filler has high intrinsic thermal conductivity and high thermal conductivity. A good thermal conductive path is formed by matching aluminum nitride powders of different particle sizes, and the thermal conductivity reaches 6W / m·K or above. Spherical aluminum nitride is selected to replace the commonly used angular crystalline silicon powder as the thermal conductive filler, which reduces the wear of the angular filler on the equipment during the production process, prolongs the service life of the machine, and reduces the metal impurities in the production process, improves the electrical properties of the molding compound, makes the product more suitable for high-power devices, and improves the reliability of the power devices.
[0017] At the same time, the present invention also provides a method for preparing a high thermal conductivity epoxy molding compound for encapsulating high-power devices. In the preparation method, a ball milling mixing method is used to disperse the curing agent, curing accelerator, release agent, toughening agent, etc. The dispersion method can achieve the same dispersion effect as the prior art, but reduces energy consumption and saves production costs.
[0018] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. DETAILED DESCRIPTION
[0019] In order to make the purpose, technical scheme and advantages of the present invention clearer, the technical scheme in the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present invention. The following embodiments are used to illustrate the present invention, but cannot be used to limit the scope of the present invention.
[0020] A high thermal conductivity epoxy molding compound for packaging high power devices, the composition and mass percentage of each component are as follows: Epoxy resin, 3%~15%; Curing agent, 1.5%~10%; Thermal conductive filler, 70%~94%; Curing accelerator, 0.05%~3%; Release agent, 0.05%~2%; Stress release agent, 0.02%~1%; Silane coupling agent, 0.1%~3%; Colorant, 0.02%~1%; Flame retardant, 0.05%~3%; Ion capture agent, 0.05%~3%; Wherein, the thermal conductive filler is composed of modified spherical aluminum nitride with different particle sizes.
[0021] In the following examples, the experimental methods used are conventional methods unless otherwise specified, and the materials, reagents, etc. used are all available from commercial sources unless otherwise specified.
[0022] The raw material formula compositions of Examples 1 to 5 are shown in Table 1: Table 1 Epoxy molding compound formula composition
[0023] Among them, the raw material formula of the high thermal conductivity epoxy molding compound for encapsulating high-power devices in Examples 1 to 5 is composed (by mass, with a total of 100 parts).
[0024] The evaluation items for the epoxy molding compound in the embodiments and comparative examples are as follows: Fluidity: Take 20g sample and measure it by injection molding machine with spiral flow metal mold, injection pressure 6.5Mpa, mold temperature 190℃±2℃.
[0025] Gelation time: Heat the electric hot plate to 175℃±1℃, take 2g~3g of sample and spread it on the iron plate, scrape it continuously with a scraper, and test the time it takes for the sample to change from fluid to gel.
[0026] The glass transition temperature (Tg) and linear expansion coefficient were tested using a thermomechanical analyzer (TMA).
[0027] Flame retardancy: vertical combustion method is adopted according to GB / T 2408 standard.
[0028] Thermal conductivity: Steady state method is used according to GB / T 10294 standard.
[0029] Example 1 A method for preparing a high thermal conductivity epoxy molding compound for encapsulating high power devices is as follows: 3.45 parts by mass of linear phenolic resin, 2.30 parts by mass of triazine phenolic resin, 0.80 parts by mass of ion scavenger hydrotalcite, 2 parts by mass of flame retardant aluminum hydroxide, 0.70 parts by mass of carnauba wax and 0.40 parts by mass of curing accelerator triphenylphosphine-1,4-benzoquinone adduct were added into a ball mill and mixed thoroughly for 1 hour to obtain mixture I.
[0030] A total of 80 parts by mass of modified spherical aluminum nitride of different particle sizes were added into a high-speed mixer in the proportion [D50 (28 μm): D50 (8 μm): D50 (3.5 μm) = 55.00:17.50:7.50], and 0.45 parts by mass of coupling agent KH-560, 0.15 parts by mass of KBM-573, 0.40 parts by mass of low stress release agent SF-8421EG and 0.30 parts by mass of carbon black were added into the high-speed mixer and mixed thoroughly for 20 minutes to obtain mixture II.
[0031] The mixture I, the mixture II, 6.15 parts by mass of o-cresol epoxy resin and 2.90 parts by mass of biphenyl melt-type epoxy resin were mixed together in a high-speed mixer to obtain an epoxy molding compound mixture.
[0032] The obtained epoxy molding compound mixture was added into a twin-screw extruder at an extrusion temperature of 80°C to obtain an epoxy resin molding compound, and its fluidity, gel time, glass transition temperature, linear expansion coefficient, flame retardancy and thermal conductivity were evaluated, as shown in Table 2.
[0033] Example 2 A method for preparing a high thermal conductivity epoxy molding compound for encapsulating high power devices is as follows: 3.00 parts by mass of linear phenolic resin, 1.17 parts by mass of triazine phenolic resin, 0.80 parts by mass of ion scavenger hydrotalcite, 1 part by mass of flame retardant aluminum hydroxide, 0.60 parts by mass of carnauba wax and 0.35 parts by mass of curing accelerator triphenylphosphine-1,4-benzoquinone adduct were added to a ball mill and mixed thoroughly for 1.5 hours to obtain mixture I.
[0034] A total of 85 parts by mass of modified spherical aluminum nitride of different particle sizes were added into a high-speed mixer in the proportion [D50 (28 μm): D50 (8 μm): D50 (3.5 μm) = 58.44:18.59:7.97], and 0.40 parts by mass of coupling agent KH-560, 0.16 parts by mass of KBM-573, 0.5 parts by mass of low stress release agent SF-8421EG and 0.32 parts by mass of carbon black were added into the high-speed mixer and mixed thoroughly for 25 minutes to obtain mixture II.
[0035] The mixture I, the mixture II, 4.20 parts by mass of o-cresol epoxy resin and 2.50 parts by mass of biphenyl melt-type epoxy resin were fully mixed together in a high-speed mixer to obtain an epoxy molding compound mixture.
[0036] The obtained epoxy molding compound mixture was added into a twin-screw extruder at an extrusion temperature of 70° C. to obtain an epoxy resin molding compound, and its fluidity, gel time, glass transition temperature, linear expansion coefficient, flame retardancy and thermal conductivity were evaluated, as shown in Table 2.
[0037] Example 3 A method for preparing a high thermal conductivity epoxy molding compound for encapsulating high power devices is as follows: 1.43 parts by mass of linear phenolic resin, 1.05 parts by mass of triazine phenolic resin, 0.80 parts by mass of ion scavenger hydrotalcite, 1 part by mass of flame retardant aluminum hydroxide, 0.45 parts by mass of carnauba wax and 0.2 parts by mass of curing accelerator triphenylphosphine-1,4-benzoquinone adduct were added to a ball mill and mixed thoroughly for 1 hour to obtain mixture I.
[0038] A total of 90 parts by mass of modified spherical aluminum nitride of different particle sizes were added into a high-speed mixer in the proportion [D50 (28 μm): D50 (8 μm): D50 (3.5 μm) = 61.88:19.69:8.44], and 0.30 parts by mass of coupling agent KH-560, 0.20 parts by mass of KBM-573, 0.35 parts by mass of low stress release agent SF-8421EG and 0.32 parts by mass of carbon black were added into the high-speed mixer and mixed thoroughly for 20 minutes to obtain mixture II.
[0039] The mixture I, the mixture II, 2.30 parts by mass of o-cresol epoxy resin and 1.60 parts by mass of biphenyl melt-type epoxy resin were mixed together in a high-speed mixer to obtain an epoxy molding compound mixture.
[0040] The obtained epoxy molding compound mixture was added into a twin-screw extruder at an extrusion temperature of 90° C. to obtain an epoxy resin molding compound, and its fluidity, gel time, glass transition temperature, linear expansion coefficient, flame retardancy and thermal conductivity were evaluated, as shown in Table 2.
[0041] Example 4 A method for preparing a high thermal conductivity epoxy molding compound for encapsulating high power devices is as follows: 2.90 parts by mass of triazine phenolic resin, 0.55 parts by mass of ion scavenger, 0.8 parts by mass of flame retardant aluminum hydroxide, 0.55 parts by mass of carnauba wax and 0.26 parts by mass of curing accelerator triphenylphosphine-1,4-benzoquinone adduct were added into a ball mill and mixed thoroughly for 2.0 hours to obtain mixture I.
[0042] A total of 89 parts by mass of modified spherical aluminum nitride of different particle sizes were added into a high-speed mixer in the proportion [D50 (28 μm): D50 (8 μm) = 70.00: 19.00], and 0.35 parts by mass of coupling agent KH-560, 0.20 parts by mass of KBM-573, 0.37 parts by mass of low stress release agent SF-8421EG and 0.32 parts by mass of carbon black were added into the high-speed mixer and mixed thoroughly for 30 minutes to obtain mixture II.
[0043] The mixture I, the mixture II, 2.80 parts by mass of biphenyl melt-type epoxy resin, and 1.90 parts by mass of biphenyl phenol-type epoxy resin were mixed together in a high-speed mixer to obtain an epoxy molding compound mixture.
[0044] The obtained epoxy molding compound mixture was added into a twin-screw extruder at an extrusion temperature of 85°C to obtain an epoxy resin molding compound, and its fluidity, gel time, glass transition temperature, linear expansion coefficient, flame retardancy and thermal conductivity were evaluated, as shown in Table 2.
[0045] Example 5 A method for preparing a high thermal conductivity epoxy molding compound for encapsulating high power devices is as follows: 2.50 parts by mass of linear phenolic resin, 0.50 parts by mass of ion scavenger, 1.0 parts by mass of flame retardant aluminum hydroxide, 0.40 parts by mass of carnauba wax and 0.20 parts by mass of curing accelerator triphenylphosphine-1,4-benzoquinone adduct were added into a ball mill and mixed thoroughly for 2.0 hours to obtain mixture I.
[0046] A total of 88.5 parts by mass of modified spherical aluminum nitride of different particle sizes were added into a high-speed mixer in the proportion [D50 (28 μm): D50 (8 μm) = 60.00: 28.50], and 0.60 parts by mass of coupling agent KH-560, 0.40 parts by mass of low stress release agent SF-8421EG and 0.30 parts by mass of carbon black were added into the high-speed mixer and mixed thoroughly for 20 minutes to obtain mixture II.
[0047] The mixture I, the mixture II, 3.20 parts by mass of dicyclopentadiene epoxy resin, and 2.40 parts by mass of biphenylphenol epoxy resin were mixed together in a high-speed mixer to obtain an epoxy molding compound mixture.
[0048] The obtained epoxy molding compound mixture was added into a twin-screw extruder at an extrusion temperature of 85°C to obtain an epoxy resin molding compound, and its fluidity, gel time, glass transition temperature, linear expansion coefficient, flame retardancy and thermal conductivity were evaluated, as shown in Table 2.
[0049] Table 2 Evaluation results of epoxy resin molding compound
[0050] Comparative Example 1 An epoxy molding compound mixture was prepared according to the component ratio and method in Example 2, except that all the modified spherical aluminum nitride in the formula was replaced by angular crystalline silicon powder according to the particle size to obtain the epoxy molding compound mixture.
[0051] Then the fluidity, gel time, glass transition temperature, linear expansion coefficient, flame retardancy and thermal conductivity were tested, as shown in Table 3.
[0052] Comparative Example 2 An epoxy molding compound mixture was prepared according to the component ratio and method in Example 3, except that all the modified spherical aluminum nitride in the formula was replaced by angular crystalline silicon powder according to the particle size to obtain an epoxy molding compound mixture.
[0053] Then the fluidity, gel time, glass transition temperature, linear expansion coefficient, flame retardancy and thermal conductivity were tested, as shown in Table 3.
[0054] Comparative Example 3 An epoxy molding compound mixture was prepared according to the component ratio and method in Example 3, except that all the modified spherical aluminum nitride in the formula was replaced by spherical aluminum oxide according to the particle size to obtain an epoxy molding compound mixture.
[0055] Then the fluidity, gel time, glass transition temperature, linear expansion coefficient, flame retardancy and thermal conductivity were tested, as shown in Table 3.
[0056] Comparative Example 4 An epoxy molding compound mixture was prepared according to the component ratio and method in Example 3, except that all the modified spherical aluminum nitride in the formula was replaced by non-modified spherical aluminum nitride according to the particle size to obtain the epoxy molding compound mixture.
[0057] Then the fluidity, gel time, glass transition temperature, linear expansion coefficient, flame retardancy and thermal conductivity were tested, as shown in Table 3.
[0058] Table 3 Epoxy molding compound test results
[0059] It can be seen from Tables 2 and 3 that the high thermal conductivity epoxy molding compound for encapsulating high-power devices provided by the present invention, the modified spherical aluminum nitride used as a thermal conductive filler in its formula composition effectively improves the thermal conductivity of the epoxy molding compound, and the thermal conductivity can reach 3.89 W / m·K when the addition amount is only 80%, which is similar to the thermal conductivity of the spherical aluminum oxide when the addition amount is 90%. When the addition amount of the modified spherical aluminum nitride reaches 90%, the thermal conductivity reaches 6.22 W / m·K, which greatly improves the thermal conductivity of the epoxy molding compound and meets the packaging requirements of higher power devices. At the same time, compared with angular crystalline silicon powder, spherical aluminum nitride avoids the problem of poor processing performance of the epoxy molding compound due to insufficient fluidity in the case of high filler.
[0060] At the same time, it can be seen from Tables 2 and 3 that the high thermal conductivity epoxy molding compound provided by the present invention for packaging high-power devices has a bending strength increased by nearly 50%, and the mechanical properties are significantly improved.
[0061] The high thermal conductivity epoxy molding compound for packaging high-power devices provided by the present invention is reasonably matched with spherical aluminum nitrides of different particle sizes, so that a higher thermal conductivity coefficient can be achieved under the condition of the same addition amount. This is because the finer spherical aluminum nitride fills the gaps between the coarse particles, making the heat conduction path more complete and achieving a higher thermal conductivity effect.
[0062] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A high thermal conductivity epoxy molding compound for encapsulating high power devices. It is characterized in that Its components and the mass percentage of each component are as follows: Epoxy resin, 3%~15%; Curing agent, 1.5%~10%; Thermal conductive filler, 70%~94%; Curing accelerator, 0.05%~3%; Release agent, 0.05%~2%; Stress release agent, 0.02%~1%; Silane coupling agent, 0.1%~3%; Colorant, 0.02%~1%; Flame retardant, 0.05%~3%; Ion capture agent, 0.05%~3%; Wherein, the thermal conductive filler is composed of modified spherical aluminum nitride with different particle sizes.
2. The high thermal conductivity epoxy molding compound for packaging high power devices as claimed in claim 1, It is characterized in that The particle size of the spherical aluminum nitride ranges from 0.5 μm to 40 μm.
3. The high thermal conductivity epoxy molding compound for packaging high power devices as claimed in claim 1, It is characterized in that The epoxy resin is at least one of o-cresol epoxy resin, cyclopentadiene epoxy resin and aromatic epoxy resin.
4. The high thermal conductivity epoxy molding compound for packaging high power devices as claimed in claim 1, It is characterized in that The curing agent is a phenolic resin curing agent; the curing agent accelerator is at least one of an imidazole accelerator, an organic phosphorus accelerator and its derivative accelerator, and a bicyclic amidine accelerator and its derivative accelerator.
5. The high thermal conductivity epoxy molding compound for packaging high power devices as claimed in claim 1, It is characterized in that The release agent is at least one of carnauba wax, montan wax and oxidized polyethylene wax.
6. The high thermal conductivity epoxy molding compound for packaging high power devices as claimed in claim 1, It is characterized in that The stress release agent is at least one of epoxidized silicone oil and epoxidized polybutadiene.
7. The high thermal conductivity epoxy molding compound for packaging high power devices as claimed in claim 1, It is characterized in that The silane coupling agent is at least one of 3-aminopropyltriethoxysilane, 3-glycidoxypropyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane, N-phenyl-3-aminopropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane.
8. The high thermal conductivity epoxy molding compound for packaging high power devices as claimed in claim 1, It is characterized in that The flame retardant is at least one of aluminum hydroxide, zinc borate, melamine cyanurate and an organophosphorus flame retardant; The ion capture agent is hydrotalcite.
9. A method for preparing a high thermal conductivity epoxy molding compound for packaging high power devices. It is characterized in that The method for preparing the high thermal conductivity epoxy molding compound for packaging high power devices according to any one of claims 1 to 8 comprises the following steps: S100, weighing a curing agent, a curing accelerator, a flame retardant, a release agent, and an ion capture agent according to the composition and the mass percentage of each component, and dispersing the weighed components by ball milling for 1 h to 2 h to obtain a mixture I; S200, uniformly mixing the modified spherical aluminum nitride filler, the silane coupling agent, the stress release agent and the colorant to obtain a mixture II; S300, uniformly mixing mixture I, mixture II and epoxy resin to obtain an epoxy molding compound mixture; S400, at a temperature of 50° C. to 100° C., extruding the epoxy molding compound mixture through a twin-screw extruder to obtain a high thermal conductivity epoxy molding compound.
10. The method for preparing the high thermal conductivity epoxy molding compound for packaging high power devices as claimed in claim 9, It is characterized in that In step S200, the modified spherical aluminum nitride thermal conductive filler is prepared by the following steps: S201, adding spherical aluminum nitride to a mixing pot, stirring and heating to 20°C to 40°C, adding deionized water to the mixing pot in batches using a spray device, collecting and testing ammonia generated by hydrolysis using a negative pressure device, and stopping adding deionized water when the hydrolysis rate of the spherical aluminum nitride is within the range of 1% to 10%; S202, adding tetraethyl orthosilicate into a mixing pot by using a spray device, the added amount being 0.2% to 5% by mass of the spherical aluminum nitride, and coating the aluminum nitride with tetraethyl orthosilicate to obtain a modified spherical aluminum nitride filler.