Expandable silicone rubber and preparation method thereof
By adding foaming agent and expandable components to the silicone rubber, low-density expandable silicone rubber is prepared, which solves the expansion and temperature increase caused by thermal runaway from the battery, and effectively protects the battery pack and avoids the shell Break and prevent the spread of heat from being controlled.
Patent Information
- Application Number
- CN202411130446.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-08
AI Technical Summary
The battery thermal runaway leads to expansion and temperature increase, and existing thermal protection components are difficult to effectively prevent the battery housing from rupturing, and their effects are limited in applications in special-shaped areas.
By adding foaming agent and expandable components to the silicone rubber, low-density expandable silicone rubber can be prepared, and a porous structure can be formed by the reaction of vinyl silicone oil, hydroxy silicone oil and hydrogen-containing silicone oil, and combined with Liquid foaming agent expands pores, improves the toughness and strength of the material, and is used for thermal protection of the battery pack.
Effectively limit battery expansion, slow down the thermal runaway speed, avoid the battery shell rupture, and prevent the spread of thermal runaway through the gradient insulation mechanism of phase change materials, significantly improving the battery's thermal protection performance.
Smart Images

Figure BDA0004997668080000051
Abstract
Description
Technical field:
[0001] The invention relates to the field of battery heat protection plates, and in particular to a low-density expandable silicone rubber and a preparation method thereof. Background technology:
[0002] With the popularization of new energy vehicles, battery thermal runaway has become a problem that needs to be solved urgently. In the early stage of thermal runaway, the battery pack will expand and the temperature will rise. Suitable thermal protection components are needed to prevent battery expansion, avoid shell rupture, and slow down the speed of runaway. Silicone rubber has good flexibility, high ductility, and certain temperature resistance and flame retardancy, so it is often used for thermal protection in special-shaped areas. Summary of the invention:
[0003] The invention provides a method for preparing low-density expandable silicone rubber, wherein a foaming agent and an expandable component are added to the silicone rubber to prepare the silicone rubber capable of secondary foaming and expansion.
[0004] The technical solution adopted by the present invention is as follows:
[0005] Vinyl silicone oil, hydroxy silicone oil, hydrogen silicone oil, a catalyst and a liquid foaming agent are stirred and mixed uniformly to obtain a mixture A;
[0006] Adding expansion components to mixture A and stirring and mixing to obtain blank material B;
[0007] The blank material B is packaged and calendered to obtain expandable silicone rubber.
[0008] In this way, when vinyl silicone oil and hydrogen silicone oil are mixed, the -SiCH=CH2 group of vinyl silicone oil and hydrogen silicone oil HSi- react under the action of catalyst to form a cross-linked silica gel network structure -SiCH2CH2Si-, which improves the overall toughness of expandable silicone rubber; at the same time, the reaction of hydrogen silicone oil and hydroxy silicone oil -SiOH can release small molecules of hydrogen, thereby generating bubbles in the colloid and providing a foaming structure. The combination of the two forms a foamed silica gel with good toughness and high strength. The liquid foaming agent can further expand the pores in the foaming structure, provide space for the secondary expansion of the expandable material, and further reduce the product density.
[0009] In some embodiments, vinyl silicone oil, hydroxy silicone oil, hydrogen silicone oil, catalyst and liquid foaming agent are mixed in a mass ratio of 30:30:(0.5-10):(0.1-2):(0.15-1);
[0010] In some embodiments, the preparation process of the mixture A includes premixing the liquid blowing agent with the hydroxy silicone oil to prepare a premix, and then adding the hydrogenated silicone oil, the catalyst, and the vinyl silicone oil to the premix;
[0011] In some embodiments, the liquid blowing agent is cyclopentane.
[0012] Thus, premixing the liquid blowing agent with the hydroxy silicone oil can make the reactants dispersed evenly.
[0013] In some embodiments, the expansion component further includes one or more of an expandable material, and / or a thickener, and / or a flame retardant, and / or a phase change material.
[0014] In some embodiments, the thickener is selected from one or more of gelatin, kaolin, bentonite, and silicon dioxide.
[0015] In some embodiments, the vinyl silicone oil is selected from a terminal vinyl silicone oil with a vinyl content of 0.01-0.1 wt % and a number average molecular weight of 1000-10000, and a high vinyl silicone oil with a vinyl content of 0.05-1 wt % and a number average molecular weight of 3000-10000.
[0016] In some embodiments, the hydroxy silicone oil is selected from one of the hydroxy silicone oils with a hydroxyl content of 5 to 10 wt %; the hydrogen-containing silicone oil is selected from one of the hydrogen-containing silicone oils with a hydrogen content of 0.5 to 1.5 wt %; and the catalyst is a platinum catalyst.
[0017] In some embodiments, the expandable material is selected from one of foamed microspheres, urea, sodium bicarbonate, and azo compounds.
[0018] In some embodiments, the flame retardant is selected from one of silicon dioxide, aluminum hydroxide, magnesium hydroxide, and glass microspheres.
[0019] In some embodiments, the phase change material is selected from paraffin and phase change microcapsules.
[0020] In some embodiments, by mass, the thickener is added in an amount of 0.1% to 20% of the mass of the mixture, the flame retardant is added in an amount of 1% to 30% of the mass of the mixture, the expandable material is added in an amount of 1% to 15% of the mass of the mixture, and the phase change material is added in an amount of 5% to 15% of the mass of the mixture;
[0021] In some embodiments, the packaging is to place the blank material B between two packaging layers, the packaging layer is a fitted double-layer structure, the inner layer is fiber cloth for tightly fitting with the blank material; the outer layer is a release film.
[0022] In some embodiments, the blank B is taken out and placed in a calendering device at a calendering temperature of 40-60° C. The blank is calendered into sheets of different thicknesses. After calendering, the expandable silicone rubber is placed in an environment of 40-60° C. for 1-12 hours.
[0023] In some embodiments, the fiber cloth is selected from one of glass fiber cloth, carbon fiber cloth, and basalt cloth.
[0024] The secondary expandable foamed silicone rubber prepared by the present invention is used for thermal protection between batteries in a battery pack. In the technical solution of the present invention, hydrogen-containing silicone oil and hydroxy silicone oil react to generate hydrogen, and the gas escapes to form a porous structure of the silicone rubber. The liquid foaming agent further enlarges the pores to provide space for the expansion of the expandable material. When the battery heats up or thermal runaway occurs, the silicone rubber expands due to the heat and squeezes the battery, limiting the expansion of the battery, avoiding rupture of the battery casing, and effectively slowing down the speed of thermal runaway of the battery. Among them, in addition to the endothermic expansion of the thermal expansion material, the phase change material can also absorb part of the heat when the battery thermally runs away, forming a gradient insulation mechanism, which prevents the thermal runaway of the battery from spreading in the battery module. Specific implementation method:
[0025] Example 1
[0026] S1. Weigh cyclopentane and hydroxy silicone oil in a mass ratio of 0.6:30, stir and mix, and obtain a hydroxy silicone oil mixed solution; the hydroxyl content in the hydroxy silicone oil is 7wt%;
[0027] S2. Weigh terminal vinyl silicone oil, hydroxyl silicone oil mixed solution, hydrogen-containing silicone oil, and platinum catalyst in a mass ratio of 30:30:5:1, place in a planetary stirrer and mix evenly to obtain a mixture A; the terminal vinyl silicone oil has a vinyl content of 0.05wt%, a number average molecular weight of 3000, and the hydrogen-containing silicone oil has a hydrogen content of 1wt%;
[0028] S3, adding gelatin, silicon dioxide, sodium bicarbonate and paraffin to mixture A according to the mass ratio of mixture A: gelatin: silicon dioxide: sodium bicarbonate: paraffin = 1:0.1:0.15:0.08:0.1, stirring and mixing to obtain blank material B;
[0029] S4, placing the blank material B into a calendering device, the upper and lower rollers of the calendering device are equipped with double-layer packaging materials, the inner layer close to the blank material B is glass fiber cloth, and the outer layer away from the blank material B is a release film. The calendering process is carried out at an equipment temperature of 50° C. to obtain a thermal insulation pad C;
[0030] S5. Place the thermal insulation pad C in a heating device at a temperature of 50° C. and cure it for 6 hours to obtain expandable silicone rubber.
[0031] Example 2
[0032] S1. Weigh cyclopentane and hydroxy silicone oil in a mass ratio of 0.15:30, stir and mix, and obtain a hydroxy silicone oil mixed solution; the hydroxyl content in the hydroxy silicone oil is 5wt%;
[0033] S2. Weigh terminal vinyl silicone oil, hydroxyl silicone oil mixed solution, hydrogen-containing silicone oil, and platinum catalyst in a mass ratio of 30:30:0.5:0.1, place in a planetary stirrer and mix evenly to obtain a mixture A; the terminal vinyl silicone oil has a vinyl content of 0.01wt%, a number average molecular weight of 2000, and the hydrogen-containing silicone oil has a hydrogen content of 0.5wt%;
[0034] S3, adding silicon dioxide, aluminum hydroxide, urea, and paraffin to the mixture A according to the mass ratio of mixture A: silicon dioxide: aluminum hydroxide: urea: paraffin = 1:0.01:0.01:0.01:0.05, stirring and mixing to obtain a blank material B;
[0035] S4, placing the blank material B into a calendering device, the upper and lower rollers of the calendering device are equipped with double-layer packaging materials, the inner layer close to the blank material B is glass fiber cloth, and the outer layer away from the blank material B is a release film. The calendering process is carried out at an equipment temperature of 40° C. to obtain a thermal insulation pad C;
[0036] S5. Place the thermal insulation pad C in a heating device at a temperature of 40° C. and cure it for 1 hour to obtain expandable silicone rubber.
[0037] Example 3
[0038] S1. Weigh cyclopentane and hydroxy silicone oil in a mass ratio of 1:30, stir and mix, and obtain a hydroxy silicone oil mixed solution; the hydroxyl content in the hydroxy silicone oil is 10wt%;
[0039] S2. Weigh high vinyl silicone oil, hydroxy silicone oil mixed solution, hydrogen-containing silicone oil, and platinum catalyst in a mass ratio of 30:30:10:2, place in a planetary stirrer and mix evenly to obtain a mixture A; the high vinyl silicone oil has a vinyl content of 1wt%, a number average molecular weight of 10000, and the hydrogen-containing silicone oil has a hydrogen content of 1.5wt%;
[0040] S3, adding bentonite, magnesium hydroxide, foaming microspheres, and phase change microcapsules to the mixture A in a mass ratio of mixture A: bentonite: magnesium hydroxide: foaming microspheres: phase change microcapsules = 1:0.2:0.3:0.15:0.15, stirring and mixing to obtain a blank B;
[0041] S4, placing the blank material B into a calendering device, the upper and lower rollers of the calendering device are equipped with double-layer packaging materials, the inner layer close to the blank material B is glass fiber cloth, and the outer layer away from the blank material B is a release film. The calendering process is carried out at an equipment temperature of 60° C. to obtain a thermal insulation pad A;
[0042] S5. Place the thermal insulation pad A in a heating device at 60° C. for curing for 12 hours to obtain expandable silicone rubber.
[0043] Comparative Example 1
[0044] The difference from Example 1 is that cyclopentane is not added, that is, step S1 does not exist, and the rest is the same as Example 1.
[0045] Comparative Example 2
[0046] The difference from Example 1 is that sodium bicarbonate is not added, that is, step S3 does not exist, and the rest is the same as Example 1.
[0047] Comparative Example 3
[0048] The difference from Example 1 is that cyclopentane and sodium bicarbonate are not added, that is, steps S1 and S3 do not exist, and the rest are the same as in Example 1.
[0049] Comparative Example 4
[0050] The difference from Example 1 is that cyclopentane, vinyl silicone oil, hydroxy silicone oil, hydrogen silicone oil, catalyst, gelatin, silicon dioxide, sodium bicarbonate and paraffin are added to the stirrer at the same time and mixed evenly, that is, steps S1, S2 and S3 are combined, and the rest are the same as Example 1.
[0051] Test method:
[0052] 1. Density: Tested in accordance with GB / T 4472-2011;
[0053] 2. Free expansion rate at 130℃: Take a sample from each group and place it on the heating platform. Turn on the heating platform and heat it to 130℃ for 20 minutes. Measure the thickness of the product after expansion and curing.
[0054] 3. Temperature resistance: Take a sample from each group and use DSC test to get the glass transition temperature of the sample;
[0055] 4. Flame retardant performance: tested in accordance with UL 94-2013;
[0056] 5. Thermal conductivity: Tested in accordance with GB 14907-2018.
[0057] Test results:
[0058]
Claims
1. A method for preparing expandable silicone rubber, characterized in that: The following steps are involved: Vinyl silicone oil, hydroxy silicone oil, hydrogen silicone oil, a catalyst and a liquid foaming agent are stirred and mixed uniformly to obtain a mixture A; Adding expansion components to mixture A and stirring and mixing to obtain blank material B; The blank material B is packaged and calendered to obtain expandable silicone rubber.
2. The method for preparing expandable silicone rubber according to claim 1, characterized in that: Vinyl silicone oil, hydroxy silicone oil, hydrogen silicone oil, catalyst and liquid foaming agent are uniformly mixed in a mass ratio of 30:30:(0.5-10):(0.1-2):(0.15-1).
3. The method for preparing expandable silicone rubber according to claim 1, characterized in that: When preparing the mixture A, the liquid blowing agent and the hydroxy silicone oil are first premixed to prepare a premix, and then the hydrogen-containing silicone oil, the catalyst and the vinyl silicone oil are added to the premix.
4. The method for preparing expandable silicone rubber according to claim 1, characterized in that: The expansion component includes one or more of an expandable material, and / or a thickener, and / or a flame retardant, and / or a phase change material.
5. The method for preparing expandable silicone rubber according to claim 1, characterized in that: The packaging is to place the blank material B between two packaging layers, the packaging layer is a fitted double-layer structure, the inner layer is a fiber cloth for tightly adhering to the blank material; the outer layer is a release film.
6. The method for preparing expandable silicone rubber according to claim 1, characterized in that: The method of placing the blank B into the packaging material for calendering also includes placing the blank B into a calendering device at a calendering temperature of 40 to 60° C., calendering the blank B into sheets of different thicknesses, and placing the expandable silicone rubber in an environment of 40 to 60° C. for 1 to 12 hours after calendering.
7. The method for preparing expandable silicone rubber according to claim 4, characterized in that: The thickener is added in an amount of 0.1% to 20% of the mass of the mixture A; the flame retardant is added in an amount of 1% to 30% of the mass of the mixture; the expandable material is added in an amount of 1% to 15% of the mass of the mixture; and the phase change material is added in an amount of 5% to 15% of the mass of the mixture.
8. The method for preparing expandable silicone rubber according to claim 1, characterized in that: The vinyl silicone oil is selected from one of a terminal vinyl silicone oil with a vinyl content of 0.01-0.1wt% and a number average molecular weight of 1000-10000 and a high vinyl silicone oil with a vinyl content of 0.05-1wt% and a number average molecular weight of 3000-10000.
9. The method for preparing expandable silicone rubber according to claim 1, characterized in that: The hydroxy silicone oil is selected from one of the hydroxy silicone oils with a hydroxyl content of 5 to 10 wt %; the hydrogen-containing silicone oil is selected from one of the hydrogen-containing silicone oils with a hydrogen content of 0.5 to 1.5 wt %; and the catalyst is a platinum catalyst.
10. A low-density expandable silicone rubber, characterized in that: The expandable silicone rubber is prepared by the preparation method of any one of claims 1 to 9.
Citation Information
Cited By
Fireproof thermal insulation material for new energy automobile battery and preparation method of fireproof thermal insulation material
CN120118519A