Rutile type titanium dioxide for color chips and production method of rutile type titanium dioxide
By simplifying the production process of rutile titanium dioxide, including salt treatment, calcination and modification treatment, the problems of high energy consumption and uneven dispersion of production are solved, efficient and low-cost titanium dioxide preparation are achieved, and the color film materials are improved Whitening and covering effects.
Patent Information
- Application Number
- CN202410951743.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-08
AI Technical Summary
The existing rutile titanium dioxide production process is complicated, resulting in high energy consumption and high cost, and uneven dispersion in the color sheet materials, affecting the whitening and covering effects.
Using salt treatment, calcination, fine crushing and modification treatment methods, including dehydration, desulfurization and crystal transformation during the calcination process, improve the dispersion performance of titanium dioxide through airflow pulverization and spraying treatment, and eliminate mortar sanding and washing and drying. Process.
It simplifies the production process, reduces energy consumption and costs, improves the dispersion performance of rutile-type titanium dioxide, and enhances its use effect in color film materials.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of color flake titanium dioxide, in particular to rutile titanium dioxide for color flakes and a production method thereof. Background Art
[0002] Color chips are a kind of hot stamping material that is made by depositing a mixed coating layer of pigment and adhesive materials on a flat and smooth object such as glass, and then peeling it off on paper after drying. It has the characteristics of pure color and not easy to reflect light. Titanium dioxide is often used in color chips, which can play the role of whitening, covering and increasing gloss, and the titanium dioxide in color chips is mostly rutile titanium dioxide. Rutile titanium dioxide refers to titanium dioxide prepared by a specific process with a structure similar to rutile minerals, which has excellent optical properties and pigment properties, as well as high UV resistance.
[0003] For example, the patent with publication number CN117327925A discloses a method for preparing rutile titanium dioxide powder by sulfuric acid method without concentration. The method uses titanium concentrate as raw material, and undergoes the steps of acid hydrolysis of titanium ore, sedimentation, filtration, ferrous sulfate crystallization, hydrolysis of external seed crystals, filtration, water washing, calcination of seed crystals, bleaching, rinsing, salt treatment, and calcination to obtain rutile titanium dioxide powder. The method does not require a concentration step, but can achieve the same production purpose, and can effectively solve the problem of high production cost of preparing titanium dioxide powder by sulfuric acid method.
[0004] However, the existing production process of rutile titanium dioxide is still relatively complicated, and the prepared rutile titanium dioxide has problems such as poor stability and uneven dispersion when used in color chips, that is, the whitening and covering effects of the color chip material are not ideal. Therefore, for the rutile titanium dioxide used in color chips, it is necessary to provide a rutile titanium dioxide production process that is more convenient to produce and has better use effects in combination with its use requirements. Summary of the invention
[0005] The technical problems to be solved by the present invention are:
[0006] The current common production process of rutile titanium dioxide is relatively complicated, resulting in high energy consumption, high time and economic costs. In addition, when rutile titanium dioxide is used in color sheet materials, it is prone to sedimentation, resulting in uneven dispersion, affecting the whitening and covering effects of rutile titanium dioxide on the material, making it difficult to meet its use requirements.
[0007] The technical solution adopted by the present invention is:
[0008] The present invention provides a method for producing rutile titanium dioxide for color sheets, comprising the following steps:
[0009] S1 Salt Treatment:
[0010] Take metatitanic acid, add desalted water, prepare the slurry, then add the salt treatment agent, mix well, and obtain the metatitanate treated slurry;
[0011] S2 Calcination:
[0012] The metatitanate treated slurry is placed in a furnace for calcination, and dehydration, desulfurization, and crystal transformation treatment are performed in sequence to obtain a crude rutile titanium dioxide product;
[0013] S3 fine crushing:
[0014] The crude rutile titanium dioxide is crushed by squeezing and then subjected to air flow milling;
[0015] S4 modification treatment:
[0016] The crushed titanium dioxide is graded and sieved to obtain titanium dioxide particles and micro titanium dioxide powder; the titanium dioxide particles are taken, an organic treatment agent is added, dispersed, and the surface of the titanium dioxide particles is sprayed with the micro titanium dioxide powder to obtain the rutile titanium dioxide.
[0017] Preferably, in step S1, the salt treating agent comprises rutile calcined seed crystals, potassium salt, phosphoric acid and aluminum salt.
[0018] Preferably, by mass, the amount of rutile calcined seed crystals is 1-7wt% of the mass of TiO2 in the slurry, the amount of potassium salt is 2-6wt% of the mass of TiO2 in the slurry, the amount of phosphoric acid is 0.5-5wt% of the mass of TiO2 in the slurry, and the amount of aluminum salt is 1-4wt% of the mass of TiO2 in the slurry.
[0019] Preferably, the TiO2 concentration in the titanate treated slurry is 280-350 g / L.
[0020] Preferably, in step S2, the dehydration temperature is 350-450°C and the dehydration time is 0.75-2h;
[0021] The desulfurization temperature is 650-720℃, and the desulfurization time is 2-2.25h;
[0022] The temperature of crystal transformation is 750-850°C, and the crystal transformation time is 1.5-2h.
[0023] Preferably, in step S3, the particle size D of the titanium dioxide after fine crushing is 90 ≤0.6μm.
[0024] Preferably, in step S4, the particle size of the titanium dioxide particles is 0.3-0.6 μm, and the particle size of the micro titanium dioxide powder is less than 0.3 μm.
[0025] Preferably, the organic treatment agent is selected from one or more of trimethylolethane, trimethylolpropane, polydimethylsiloxane, hydroxy silicone oil, hydrogenated silicone oil, alkyl-modified silicone oil and silane coupling agent, and the amount of the organic treatment agent is 1-10wt‰ of the mass of TiO2 in titanium dioxide.
[0026] Preferably, during the spray treatment, the micro titanium dioxide powder is placed in a solvent, mixed, and the mixed slurry is sprayed; after spraying, the solvent is removed by evaporation and drying.
[0027] The beneficial effects of the present invention are as follows:
[0028] The present invention can achieve high production efficiency while ensuring product performance after eliminating the process steps of beating sand milling, inorganic coating, washing and drying in the traditional preparation process, that is, it has the advantages of short production process, low energy consumption and low production cost. After the crude rutile titanium dioxide is prepared, the particle size of the titanium dioxide is adjusted and sorted, and titanium dioxide with different particle sizes is processed to form a connection and combination, change the surface morphology and structure of the titanium dioxide particles, reduce the surface energy of the titanium dioxide particles, thereby improving the problem of easy sedimentation and poor dispersion effect, and improving the dispersion performance of the rutile titanium dioxide when used in the color sheet material. DETAILED DESCRIPTION
[0029] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0030] The present invention provides a method for producing rutile titanium dioxide for color chips, which can omit the process steps of beating sand milling, inorganic coating, washing and drying in the traditional preparation process, and has the advantages of short production process, low energy consumption, low production cost, etc., and specifically comprises the following steps:
[0031] (1) Salt treatment
[0032] Take a metatitanic acid raw material, control the iron content therein to meet Fe2O3≤30ppm, add desalted water for washing, adjust the slurry concentration to meet TiO2 of 280-350g / L, then add a salt treatment agent, and the amount of the salt treatment agent added is calculated and adjusted according to the total mass of TiO2 in the slurry to obtain a metatitanic acid salt treated slurry;
[0033] Among them, the salt treatment agent includes rutile calcined seeds, potassium salts, phosphoric acid and aluminum salts. Specifically, the rutile calcined seeds account for 1-7wt% of the titanium raw material (calculated as TiO2), the potassium salt can be selected from any one or more of potassium hydroxide, potassium carbonate, potassium sulfate, potassium chloride, etc., and the potassium salt (calculated as K2O) accounts for 2-6wt% of the titanium raw material (calculated as TiO2), the phosphoric acid (calculated as P2O5) accounts for 0.5-5wt% of the titanium raw material (calculated as TiO2), the aluminum salt can be selected from any one or more of aluminum hydroxide, aluminum sulfate, sodium aluminate, etc., and the aluminum salt (calculated as Al2O3) accounts for 1-4wt% of the titanium raw material (calculated as TiO2).
[0034] (2) Calcination
[0035] The titanate-treated slurry is dehydrated by a diaphragm press and then sent to a rotary kiln for calcination at 750-850°C for 3-10h. The specific process is: dehydration at 350-450°C for 0.75-2h, desulfurization at 650-720°C for 2-2.25h, and crystal transformation at 750-850°C for 1.5-2h to obtain a crude rutile titanium dioxide.
[0036] (3) Crushing
[0037] The crude rutile titanium dioxide is first crushed by roller mill, and the operating parameters are: feed rate 1.5-3.0 tons / hour, roller extrusion pressure 15-18MPa; then fully ground, depolymerized and dispersed by Raymond mill, and the operating parameters are: feed rate 1.5-2.5 tons / hour, analyzer current 80-130A, fan frequency 30-45Hz; and the initially crushed titanium dioxide is obtained, and the initially crushed titanium dioxide should meet the following requirements: 325 mesh sieve residue content ≤0.01%;
[0038] The initially crushed titanium dioxide is then pulverized with superheated steam as the pulverizing medium and subjected to air flow pulverization to achieve deep deagglomeration. The operating parameters are: pulverizing steam pressure 14-23MPa, temperature 260-330℃, powder feed 1.5-3.5 tons / hour, laser particle size analyzer detection D 90 ≤0.6μm.
[0039] (4) Modification treatment
[0040] The crushed titanium dioxide is graded and sieved to obtain titanium dioxide particles with a particle size of 0.3-0.6 μm and micro titanium dioxide powder with a particle size of less than 0.3 μm; the titanium dioxide particles are taken, an organic treatment agent is added, and uniformly dispersed; the micro titanium dioxide powder is mixed with a solvent, and the surface of the titanium dioxide particles is modified by spraying, and dried to obtain rutile titanium dioxide;
[0041] Among them, the organic treatment agent can be selected from one or more of trimethylolethane, trimethylolpropane, polydimethylsiloxane, hydroxy silicone oil, hydrogenated silicone oil, alkyl-modified silicone oil and silane coupling agent, and the addition amount of the organic treatment agent calculated as TiO2 is 1-10wt‰; the solvent can be selected from any one of ethanol, acetone and ether.
[0042] Example 1
[0043] Step 1: Use titanic acid as raw material and wash it twice with pure water. The raw material titanic acid must satisfy the requirement that Fe2O3 ≤ 30ppm; add desalted water and mix well to make the slurry concentration about 300g / L; then add a salt treatment agent prepared by mixing rutile calcined seeds, potassium hydroxide, phosphoric acid and aluminum hydroxide, mix well to obtain titanate treated slurry, and the rutile calcined seeds must be controlled to be 4wt% of the mass of TiO2 in the titanium salt slurry, potassium hydroxide to be 4.2wt% of the mass of TiO2 in the titanium salt slurry, phosphoric acid to be 2.7wt% of the mass of TiO2 in the titanium salt slurry, and aluminum hydroxide to be 2.6wt% of the mass of TiO2 in the titanium salt slurry.
[0044] Step 2: Use a diaphragm press to dehydrate the titanate-treated slurry, send it into a rotary kiln, heat and calcine it, and dehydrate it at 350±5℃ for 1h, desulfurize it at 705±5℃ for 2.25h, and transform it into a crystal form at 850℃ for 1.75h to obtain a crude rutile titanium dioxide with a high blue phase.
[0045] Step 3: The crude rutile titanium dioxide is first crushed by roller mill, the feed rate of roller mill is controlled to be 2.5 tons / hour, the roller extrusion pressure is 18MPa, and then it is fully ground by Raymond mill, the feed rate of Raymond mill is controlled to be 2 tons / hour, the current of analyzer is 110A, the fan frequency is 40Hz, and the content of 325 mesh residue is ≤0.01%; then superheated steam is used as the crushing medium to air flow crush the rutile titanium dioxide to make it deeply depolymerized, the crushing steam pressure of air flow crushing is 20MPa, the temperature is 280℃, and the powder feed amount is 2.5 tons / hour. After crushing, it is detected by laser particle size analyzer until the titanium dioxide D 90 ≤0.6μm.
[0046] Step 4: grade and screen the crushed titanium dioxide to separate titanium dioxide particles with a particle size of 0.3-0.6μm and micro titanium dioxide powder with a particle size less than 0.3μm; take the titanium dioxide particles, add trimethylolethane, the trimethylolethane accounts for 5wt% of TiO2 in the titanium dioxide particles, and disperse them evenly; mix the micro titanium dioxide powder with ethanol to form a slurry, and coat the micro titanium dioxide powder slurry on the surface of the titanium dioxide particles by fluidized spray, and evaporate and dry to obtain rutile titanium dioxide.
[0047] The L value, b value, tinting power (TCS value) and base color tone (Scx value) of the above rutile titanium dioxide were measured using the measurement methods of GB / T 1706-2006 and GB / T 5211.16-2007. The results are shown in Table 1 below:
[0048] Table 1 Performance test results of rutile titanium dioxide prepared in Example 1
[0049] Comparison Items L value b-value TCS value Scx value Example 1 98.2 1.75 2130 4.65
[0050] Example 2
[0051] Step 1: Use titanic acid as raw material and wash it twice with pure water. The raw material titanic acid must satisfy the requirement that Fe2O3 ≤ 30ppm; add desalted water and mix well to make the slurry concentration about 300g / L; then add a salt treatment agent prepared by mixing rutile calcined seeds, potassium hydroxide, phosphoric acid and aluminum hydroxide, mix well to obtain titanate treated slurry, and the rutile calcined seeds must be controlled to be 4wt% of the mass of TiO2 in the titanium salt slurry, potassium hydroxide to be 4.2wt% of the mass of TiO2 in the titanium salt slurry, phosphoric acid to be 2.7wt% of the mass of TiO2 in the titanium salt slurry, and aluminum hydroxide to be 2.6wt% of the mass of TiO2 in the titanium salt slurry.
[0052] Step 2: Use a diaphragm press to dehydrate the titanate-treated slurry, send it into a rotary kiln, heat and calcine it, and dehydrate it at 350±5℃ for 1h, desulfurize it at 705±5℃ for 2.25h, and transform it into a crystal form at 850℃ for 1.75h to obtain a crude rutile titanium dioxide with a high blue phase.
[0053] Step 3: The crude rutile titanium dioxide is first crushed by roller mill, the feed rate of roller mill is controlled to be 2.5 tons / hour, the roller extrusion pressure is 18MPa, and then it is fully ground by Raymond mill, the feed rate of Raymond mill is controlled to be 2 tons / hour, the current of analyzer is 110A, the fan frequency is 40Hz, and the content of 325 mesh residue is ≤0.01%; then superheated steam is used as the crushing medium to air flow crush the rutile titanium dioxide to make it deeply depolymerized, the crushing steam pressure of air flow crushing is 20MPa, the temperature is 280℃, and the powder feed amount is 2.5 tons / hour. After crushing, it is detected by laser particle size analyzer until the titanium dioxide D 90 ≤0.6μm.
[0054] Step 4: grade and screen the crushed titanium dioxide to separate titanium dioxide particles with a particle size of 0.3-0.6μm and micro titanium dioxide powder with a particle size less than 0.3μm; take the titanium dioxide particles, add trimethylolethane, the trimethylolethane accounts for 2wt% of TiO2 in the titanium dioxide particles, and disperse them evenly; mix the micro titanium dioxide powder with ethanol to form a slurry, and coat the micro titanium dioxide powder slurry on the surface of the titanium dioxide particles by fluidized spray, and evaporate and dry to obtain rutile titanium dioxide.
[0055] In the same manner as in Example 1, the L value, b value, tinting power (TCS value) and base color tone (Scx value) of the above rutile titanium dioxide were measured. The results are shown in Table 1 below:
[0056] Table 1 Performance test results of rutile titanium dioxide prepared in Example 1
[0057] Comparison Items L value b-value TCS value Scx value Example 1 97.0 1.68 2015 4.47
[0058] Example 3
[0059] Step 1: Use titanic acid as raw material and wash it twice with pure water. The raw material titanic acid must satisfy the requirement that Fe2O3 ≤ 30ppm; add desalted water and mix well to make the slurry concentration about 300g / L; then add a salt treatment agent prepared by mixing rutile calcined seeds, potassium hydroxide, phosphoric acid and aluminum hydroxide, mix well to obtain titanate treated slurry, and the rutile calcined seeds must be controlled to be 4wt% of the mass of TiO2 in the titanium salt slurry, potassium hydroxide to be 4.2wt% of the mass of TiO2 in the titanium salt slurry, phosphoric acid to be 2.7wt% of the mass of TiO2 in the titanium salt slurry, and aluminum hydroxide to be 2.6wt% of the mass of TiO2 in the titanium salt slurry.
[0060] Step 2: Use a diaphragm press to dehydrate the titanate-treated slurry, send it into a rotary kiln, heat and calcine it, and dehydrate it at 350±5℃ for 1h, desulfurize it at 705±5℃ for 2.25h, and transform it into a crystal form at 850℃ for 1.75h to obtain a crude rutile titanium dioxide with a high blue phase.
[0061] Step 3: The crude rutile titanium dioxide is first crushed by roller mill, the feed rate of roller mill is controlled to be 2.5 tons / hour, the roller extrusion pressure is 18MPa, and then it is fully ground by Raymond mill, the feed rate of Raymond mill is controlled to be 2 tons / hour, the current of analyzer is 110A, the fan frequency is 40Hz, and the content of 325 mesh residue is ≤0.01%; then superheated steam is used as the crushing medium to air flow crush the rutile titanium dioxide to make it deeply depolymerized, the crushing steam pressure of air flow crushing is 20MPa, the temperature is 280℃, and the powder feed amount is 2.5 tons / hour. After crushing, it is detected by laser particle size analyzer until the titanium dioxide D 90 ≤0.6μm.
[0062] Step 4: grade and screen the crushed titanium dioxide to separate titanium dioxide particles with a particle size of 0.3-0.6μm and micro titanium dioxide powder with a particle size less than 0.3μm; take the titanium dioxide particles, add trimethylolethane, the trimethylolethane accounts for 8.7wt% of TiO2 in the titanium dioxide particles, and disperse them evenly; mix the micro titanium dioxide powder with ethanol to form a slurry, and coat the micro titanium dioxide powder slurry on the surface of the titanium dioxide particles by fluidized spray, and evaporate and dry to obtain rutile titanium dioxide.
[0063] In the same manner as in Example 1, the L value, b value, tinting power (TCS value) and base color tone (Scx value) of the above rutile titanium dioxide were measured. The results are shown in Table 1 below:
[0064] Table 1 Performance test results of rutile titanium dioxide prepared in Example 1
[0065] Comparison Items L value b-value TCS value Scx value Example 1 98.0 1.74 2125 4.66
[0066] Example 4
[0067] Step 1: Use titanic acid as raw material and wash it twice with pure water. The raw material titanic acid must satisfy the requirement that Fe2O3 ≤ 30ppm; add desalted water and mix well to make the slurry concentration about 300g / L; then add a salt treatment agent prepared by mixing rutile calcined seeds, potassium hydroxide, phosphoric acid and aluminum hydroxide, mix well to obtain titanate treated slurry, and the rutile calcined seeds must be controlled to be 4wt% of the mass of TiO2 in the titanium salt slurry, potassium hydroxide to be 4.2wt% of the mass of TiO2 in the titanium salt slurry, phosphoric acid to be 2.7wt% of the mass of TiO2 in the titanium salt slurry, and aluminum hydroxide to be 2.6wt% of the mass of TiO2 in the titanium salt slurry.
[0068] Step 2: Use a diaphragm press to dehydrate the titanate-treated slurry, send it into a rotary kiln, heat and calcine it, and dehydrate it at 350±5℃ for 1h, desulfurize it at 705±5℃ for 2.25h, and transform it into a crystal form at 850℃ for 1.75h to obtain a crude rutile titanium dioxide with a high blue phase.
[0069] Step 3: The crude rutile titanium dioxide is first crushed by roller mill, the feed rate of roller mill is controlled to be 2.5 tons / hour, the roller extrusion pressure is 18MPa, and then it is fully ground by Raymond mill, the feed rate of Raymond mill is controlled to be 2 tons / hour, the current of analyzer is 110A, the fan frequency is 40Hz, and the content of 325 mesh residue is ≤0.01%; then superheated steam is used as the crushing medium to air flow crush the rutile titanium dioxide to make it deeply depolymerized, the crushing steam pressure of air flow crushing is 20MPa, the temperature is 280℃, and the powder feed amount is 2.5 tons / hour. After crushing, it is detected by laser particle size analyzer until the titanium dioxide D 90 ≤0.6μm.
[0070] Step 4: grade and screen the crushed titanium dioxide to separate titanium dioxide particles with a particle size of 0.3-0.6μm and micro titanium dioxide powder with a particle size less than 0.3μm; take the titanium dioxide particles, add an equal mass of a mixed treatment agent of trimethylolethane, polydimethylsiloxane and hydroxy silicone oil, the mixed treatment agent accounts for 5wt% of TiO2 in the titanium dioxide particles, and disperse them evenly; mix the micro titanium dioxide powder with ethanol to form a slurry, and coat the micro titanium dioxide powder slurry on the surface of the titanium dioxide particles by fluidized spray, and evaporate and dry to obtain rutile titanium dioxide.
[0071] In the same manner as in Example 1, the L value, b value, tinting power (TCS value) and base color tone (Scx value) of the above rutile titanium dioxide were measured. The results are shown in Table 1 below:
[0072] Table 1 Performance test results of rutile titanium dioxide prepared in Example 1
[0073] Comparison Items L value b-value TCS value Scx value Example 1 97.9 1.78 2143 4.58
[0074] Comparative Example 1
[0075] Step 1: Use titanic acid as raw material and wash it twice with pure water. The raw material titanic acid must satisfy the requirement that Fe2O3 ≤ 30ppm; add desalted water and mix well to make the slurry concentration about 300g / L; then add a salt treatment agent prepared by mixing rutile calcined seeds, potassium hydroxide, phosphoric acid and aluminum hydroxide, mix well to obtain titanate treated slurry, and the rutile calcined seeds must be controlled to be 4wt% of the mass of TiO2 in the titanium salt slurry, potassium hydroxide to be 4.2wt% of the mass of TiO2 in the titanium salt slurry, phosphoric acid to be 2.7wt% of the mass of TiO2 in the titanium salt slurry, and aluminum hydroxide to be 2.6wt% of the mass of TiO2 in the titanium salt slurry.
[0076] Step 2: Use a diaphragm press to dehydrate the titanate-treated slurry, send it into a rotary kiln, heat and calcine it, and dehydrate it at 350±5℃ for 1h, desulfurize it at 705±5℃ for 2.25h, and transform it into a crystal form at 850℃ for 1.75h to obtain a crude rutile titanium dioxide with a high blue phase.
[0077] Step 3: The crude rutile titanium dioxide is first crushed by roller mill, the feed rate of roller mill is controlled to be 2.5 tons / hour, the roller extrusion pressure is 18MPa, and then it is fully ground by Raymond mill, the feed rate of Raymond mill is controlled to be 2 tons / hour, the current of analyzer is 110A, the fan frequency is 40Hz, and the content of 325 mesh residue is ≤0.01%; then superheated steam is used as the crushing medium to air flow crush the rutile titanium dioxide to make it deeply depolymerized, the crushing steam pressure of air flow crushing is 20MPa, the temperature is 280℃, and the powder feed amount is 2.5 tons / hour. After crushing, it is detected by laser particle size analyzer until the titanium dioxide D 90 ≤0.6μm.
[0078] Step 4: Add trimethylolethane to the crushed titanium dioxide, the trimethylolethane accounting for 5wt% of TiO2 in the titanium dioxide particles, disperse evenly, dry and granulate to obtain rutile titanium dioxide.
[0079] In the same manner as in Example 1, the L value, b value, tinting power (TCS value) and base color tone (Scx value) of the above rutile titanium dioxide were measured. The results are shown in Table 1 below:
[0080] Table 1 Performance test results of rutile titanium dioxide prepared in Example 1
[0081] Comparison Items L value b-value TCS value Scx value Example 1 96.2 1.47 1980 4.02
[0082] Comparative Example 2
[0083] Step 1: Use titanic acid as raw material and wash it twice with pure water. The raw material titanic acid must satisfy the requirement that Fe2O3 ≤ 30ppm; add desalted water and mix well to make the slurry concentration about 300g / L; then add a salt treatment agent prepared by mixing rutile calcined seeds, potassium hydroxide, phosphoric acid and aluminum hydroxide, mix well to obtain titanate treated slurry, and the rutile calcined seeds must be controlled to be 4wt% of the mass of TiO2 in the titanium salt slurry, potassium hydroxide to be 4.2wt% of the mass of TiO2 in the titanium salt slurry, phosphoric acid to be 2.7wt% of the mass of TiO2 in the titanium salt slurry, and aluminum hydroxide to be 2.6wt% of the mass of TiO2 in the titanium salt slurry.
[0084] Step 2: Use a diaphragm press to dehydrate the titanate-treated slurry, send it into a rotary kiln, heat and calcine it, and dehydrate it at 350±5℃ for 1h, desulfurize it at 705±5℃ for 2.25h, and transform it into a crystal form at 850℃ for 1.75h to obtain a crude rutile titanium dioxide with a high blue phase.
[0085] Step 3: Firstly, the crude rutile titanium dioxide is crushed by roller mill, and the feed rate of roller mill is controlled to be 2.5 tons / hour and the roller extrusion pressure is 30MPa. After crushing, it is tested by laser particle size analyzer until the titanium dioxide D 90 ≤0.6μm.
[0086] Step 4: Add trimethylolethane to the crushed titanium dioxide, the trimethylolethane accounting for 5wt% of TiO2 in the titanium dioxide particles, disperse evenly, dry and granulate to obtain rutile titanium dioxide.
[0087] In the same manner as in Example 1, the L value, b value, tinting power (TCS value) and base color tone (Scx value) of the above rutile titanium dioxide were measured. The results are shown in Table 1 below:
[0088] Table 1 Performance test results of rutile titanium dioxide prepared in Example 1
[0089] Comparison Items L value b-value TCS value Scx value Example 1 95.5 1.41 1925 3.88
[0090] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for producing rutile titanium dioxide for color sheets, It is characterized in that The steps include: S1 Salt Treatment: Take metatitanic acid, add desalted water, prepare the slurry, then add the salt treatment agent, mix well, and obtain the metatitanate treated slurry; S2 Calcination: The metatitanate treated slurry is placed in a furnace for calcination, and dehydration, desulfurization, and crystal transformation treatment are performed in sequence to obtain a crude rutile titanium dioxide product; S3 fine crushing: The crude rutile titanium dioxide is crushed by squeezing and then subjected to air flow milling; S4 modification treatment: The crushed titanium dioxide is graded and sieved to obtain titanium dioxide particles and micro titanium dioxide powder; the titanium dioxide particles are taken, an organic treatment agent is added, dispersed, and the surface of the titanium dioxide particles is sprayed with the micro titanium dioxide powder to obtain the rutile titanium dioxide.
2. The method for producing rutile titanium dioxide for color flakes according to claim 1, It is characterized in that In step S1, the salt treatment agent includes rutile calcined seed crystals, potassium salt, phosphoric acid and aluminum salt.
3. The method for producing rutile titanium dioxide for color flakes according to claim 2, It is characterized in that By mass, the amount of rutile calcined seed is the amount of TiO 2 The amount of potassium salt is 1-7wt% of the mass of TiO 2 The amount of phosphoric acid used is 2-6wt% of the mass of TiO 2 The amount of aluminum salt is 0.5-5wt% of the mass of TiO 2 1-4wt% of mass.
4. The method for producing rutile titanium dioxide for color flakes according to claim 3, It is characterized in that Titanate treatment of TiO in slurry 2 The concentration is 280-350g / L.
5. The method for producing rutile titanium dioxide for color flakes according to claim 1, It is characterized in that In step S2, the dehydration temperature is 350-450°C and the dehydration time is 0.75-2h; The desulfurization temperature is 650-720℃, and the desulfurization time is 2-2.25h; The temperature of crystal transformation is 750-850°C, and the crystal transformation time is 1.5-2h.
6. The method for producing rutile titanium dioxide for color flakes according to claim 1, It is characterized in that In step S3, the particle size of the titanium dioxide after fine crushing is D 90 ≤0.6μm.
7. The method for producing rutile titanium dioxide for color flakes according to any one of claims 1 to 6, It is characterized in that In step S4, the particle size of the titanium dioxide particles is 0.3-0.6 μm, and the particle size of the micro titanium dioxide powder is less than 0.3 μm.
8. The method for producing rutile titanium dioxide for color flakes according to claim 7, It is characterized in that The organic treatment agent is selected from one or more of trimethylolethane, trimethylolpropane, polydimethylsiloxane, hydroxy silicone oil, hydrogen silicone oil, alkyl modified silicone oil and silane coupling agent, and the amount of the organic treatment agent is 2 1-10wt‰ of mass.
9. The method for producing rutile titanium dioxide for color flakes according to claim 7, It is characterized in that During the spray treatment, the micro titanium dioxide powder is placed in a solvent, mixed, and the mixed slurry is sprayed; after spraying, the solvent is removed by evaporation and drying.
10. Rutile titanium dioxide for color flakes prepared by the production method according to any one of claims 1 to 9.