Marine antifouling paint and preparation method thereof

Through the combination of graphene modified organic boron antifouling agent and other materials, a non-toxic and environmentally friendly marine antifouling coating was prepared, which solved the problem of damage to the marine ecological chain by existing marine antifouling coatings and achieved efficient Anti-fouling performance and low usage meet the anti-fouling needs of marine equipment.

CN118909496AActive Publication Date: 2024-11-08HUBEI INST OF AEROSPACE CHEMOTECHNOLOGY
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411165366.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-08
Estimated Expiration
2044-08-23

AI Technical Summary

Technical Problem

Existing marine antifouling coatings cause damage to the marine ecological chain, especially those that are toxic or may cause damage to the marine biological chain, are restricted, and a non-toxic, environmentally friendly and long-term antifouling alternative is needed.

Method used

Graphene modified organic boron antifouling agent is used as the main antifouling agent, and graphene modified organic with high antifouling properties is prepared by adding xylene, graphene oxide and pyridine triphenyl boron to the reaction device. Boron antifouling agent and mix it with zinc acrylate self-polishing resin, rosin, zinc oxide, titanium oxide, iron oxide, organic bentonite and talc to prepare marine antifouling coatings.

Benefits of technology

The marine antifouling coating has comprehensive antifouling properties. Graphene modified organic boron antifouling agent can be more effectively adsorbed on dirty biological surfaces, improve the use rate of antifouling agents, reduce the amount of antifouling agents, and is not suitable for the ocean The ecological chain causes damage to meet the pollution prevention needs of all types of marine equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118909496A_ABST
    Figure CN118909496A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of marine coatings, and particularly discloses a marine antifouling coating and a preparation method thereof.The marine antifouling coating comprises, by weight, 100 parts of zinc acrylate self-polishing resin; 50 to 150 parts of rosin; 80 to 120 parts of a graphene modified organic boron antifouling agent; 50 to 80 parts of copper pyrithione; 20 to 50 parts of zinc oxide; 5-15 parts of titanium oxide; 5-15 parts of iron oxide; 5 to 15 parts of organic bentonite; 5 to 15 parts of talcum powder; 150 to 250 parts of xylene; the preparation method of the graphene modified organic boron antifouling agent comprises the following steps: adding xylene, graphene oxide and pyridine triphenyl boron into a reaction device, and reacting to obtain the graphene modified organic boron antifouling agent. The coating takes the graphene modified organic boron antifouling agent as a main antifouling agent, and has comprehensive antifouling performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of marine coatings, and in particular to a marine antifouling coating and a preparation method thereof. Background Art

[0002] Ever since humans began to set foot in the ocean, they have begun to explore marine anti-fouling technology in response to a series of serious problems caused by the attachment of marine fouling organisms to ship hulls.

[0003] In the past few decades, organotin antifouling agents have been the first choice for various antifouling coatings due to their excellent antifouling effect; however, as the impact of organotin on the marine ecological environment has gradually become apparent, the use of organotin antifouling agents has been banned. With the ban on the use of organotin antifouling coatings, self-polishing antifouling coatings using cuprous oxide as a biocidal agent have gradually become the mainstream product of antifouling coatings; however, when the copper ion content in seawater is too high, it will also damage the ecological chain of marine organisms. With the increasing global calls for marine environmental protection and the increasing awareness of energy conservation, the use of toxic or destructive coatings to the marine biological chain is subject to more and more restrictions and will eventually be eliminated, making non-toxic, environmentally friendly and long-lasting antifouling coatings more and more widely concerned. Summary of the invention

[0004] In view of the above problems, the first object of the present invention is to provide a marine antifouling coating, which uses a graphene-modified organic boron antifouling agent as a main antifouling agent and has comprehensive antifouling properties.

[0005] The second object of the present invention is to provide a method for preparing the above-mentioned marine antifouling coating.

[0006] The first technical solution adopted by the present invention is: a marine antifouling paint, comprising the following components by weight:

[0007] 100 parts of zinc acrylate self-polishing resin;

[0008] 50-150 parts of rosin;

[0009] 80-120 parts of graphene-modified organic boron antifouling agent;

[0010] 50-80 parts of copper pyrithione;

[0011] 20-50 parts of zinc oxide;

[0012] 5-15 parts of titanium oxide;

[0013] 5-15 parts of iron oxide;

[0014] 5-15 parts of organic bentonite;

[0015] 5-15 parts of talcum powder;

[0016] 150-250 parts of xylene;

[0017] The graphene-modified organic boron antifouling agent is prepared by the following method:

[0018] Xylene, graphene oxide and pyridine triphenyl boron are added into a reaction device for reaction to obtain a graphene-modified organic boron antifouling agent.

[0019] Preferably, the number average molecular weight of the zinc acrylate self-polishing resin is 2000-3000.

[0020] Preferably, the mass percentage content of Zn in the zinc acrylate self-polishing resin is 6% to 7%.

[0021] Preferably, the graphene-modified organic boron antifouling agent is prepared by the following method:

[0022] S1: adding xylene, graphene oxide and pyridine triphenylborane into a reaction device, stirring and heating to react; stopping the reaction until the precipitate obtained after centrifugal separation of the solution does not show stratification, and obtaining a reaction solution;

[0023] S2: The reaction solution is filtered and dried to obtain a graphene-modified organic boron antifouling agent.

[0024] Preferably, the amount of xylene used is 1 / 3 to 2 / 3 of the capacity of the reaction device.

[0025] Preferably, the step S1 comprises: adding xylene, graphene oxide and pyridine triphenyl boron into a reaction device, stirring and heating to 50° C. to 90° C.

[0026] Preferably, the mass ratio of graphene oxide to pyridine triphenyl boron is 1:(1-3).

[0027] Preferably, the acid value of the graphene oxide is 500-600 mgKOH / g.

[0028] The second technical solution adopted by the present invention is: a method for preparing the marine antifouling coating as described in the first technical solution, comprising the following steps:

[0029] S10: weigh each component and set aside;

[0030] S20: Fully mix and grind zinc acrylate self-polishing resin, rosin, graphene-modified organic boron antifouling agent, copper pyrithione, zinc oxide, titanium oxide, iron oxide, organic bentonite, talcum powder and xylene, filter and obtain the marine antifouling coating after the particle size is less than 50 μm.

[0031] Beneficial effects of the above technical solution:

[0032] (1) The marine antifouling coating disclosed in the present invention uses graphene-modified organic boron antifouling agent as the main antifouling agent and has comprehensive antifouling performance.

[0033] (2) Compared with the graphene and organic boron composites in the prior art, the graphene-modified organic boron antifouling agent prepared by the preparation method provided by the present invention can better exert the antifouling effect of organic boron and graphene at the same time and has better antifouling performance.

[0034] (3) The marine antifouling coating provided by the present invention uses graphene-modified organic boron antifouling agent as the main antifouling agent. When the graphene-modified organic boron antifouling agent is dissolved in seawater, based on the huge specific surface area of ​​graphene, the antifouling agent can be more easily adsorbed on the surface of fouling organisms to play an antifouling role, thereby increasing the utilization rate of the antifouling agent and thus reducing the amount of antifouling agent used.

[0035] (4) The marine antifouling coating provided by the present invention uses graphene-modified organic boron as the main antifouling agent, which not only exerts the antifouling effects of graphene and organic boron at the same time, but also, based on the huge surface area of ​​the graphene sheet, it is easier to adsorb on the surface of fouling organisms, effectively improving the utilization rate of the organic boron antifouling agent and reducing the amount of the antifouling agent. The antifouling paint prepared by this method has excellent antifouling ability and good physical properties, and can meet the antifouling needs of various types of marine engineering equipment. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 The present invention is a process flow chart of a method for preparing a marine antifouling coating. DETAILED DESCRIPTION

[0037] The present invention is further described below through specific embodiments. It should be pointed out that, for ordinary technicians in this field, several modifications and improvements can be made without departing from the principle of the present invention, and these should also be regarded as belonging to the protection scope of the present invention.

[0038] The contents not described in detail in the specification of the present invention belong to the common knowledge of professionals in the field.

[0039] The present invention discloses a marine antifouling coating, which comprises the following components by weight:

[0040] 100 parts of zinc acrylate self-polishing resin; 50-150 parts of rosin; 80-120 parts of graphene-modified organic boron antifouling agent; 50-80 parts of copper pyrithione; 20-50 parts of zinc oxide; 5-15 parts of titanium oxide; 5-15 parts of iron oxide; 5-15 parts of organic bentonite; 5-15 parts of talc; and 150-250 parts of xylene.

[0041] The number average molecular weight of the zinc acrylate self-polishing resin is 2000-3000, and the mass percentage content of Zn in the zinc acrylate self-polishing resin is 6%-7%.

[0042] The graphene-modified organic boron antifouling agent is prepared by the following method:

[0043] S1: Add 1 / 3 to 2 / 3 of the capacity of xylene, graphene oxide and pyridine triphenyl boron into a reaction device (such as a flask), stir and heat to 50° C. to 90° C. to react; stop the reaction until the precipitate obtained after centrifugal separation of the solution does not show stratification (after reacting for a period of time, take a small amount of solution in the reaction device and centrifuge to obtain a precipitate. When the precipitate does not show stratification, stop the reaction to obtain a reaction solution), and obtain a reaction solution;

[0044] The acid value of the graphene oxide is (500-600) mgKOH / g; the mass ratio of graphene oxide to pyridine triphenyl boron is 1:(1-3);

[0045] S2: The reaction solution is filtered and dried to obtain a graphene-modified organic boron antifouling agent.

[0046] like Figure 1 As shown, the marine antifouling coating is prepared by the following steps:

[0047] S10: Accurately weigh each component in a dry environment and set aside;

[0048] S20: Fully mix and grind zinc acrylate self-polishing resin, rosin, graphene-modified organic boron antifouling agent, copper pyrithione, zinc oxide, titanium oxide, iron oxide, organic bentonite, talcum powder and xylene, filter and obtain the marine antifouling coating after the particle size is less than 50 μm.

[0049] The prepared marine antifouling coating was subjected to a shallow sea immersion test in the sea area according to GB / T 5370.

[0050] Example 1

[0051] Preparation of graphene-modified organic boron antifouling agent:

[0052] S1: Add 300 mL of xylene, 1 part by weight of graphene oxide and 3 parts by weight of pyridine triphenyl boron into a 500 mL flask, stir and heat to 90°C to react; after reacting for 2 hours, take 5 mL of the reaction solution and centrifuge to obtain a precipitate, and stop the reaction when the precipitate does not show stratification to obtain a reaction solution; wherein the acid value of the graphene oxide is (500-600) mgKOH / g;

[0053] S2: The reaction solution is filtered and dried to obtain a graphene-modified organic boron antifouling agent.

[0054] Preparation of marine antifouling coatings:

[0055] Weigh 100 parts of zinc acrylate self-polishing resin, 50 parts of rosin, 80 parts of graphene-modified organic boron antifouling agent, 80 parts of copper pyrithione, 50 parts of zinc oxide, 5 parts of titanium oxide, 5 parts of iron oxide, 15 parts of organic bentonite, 10 parts of talc and 150 parts of xylene respectively;

[0056] Zinc acrylate self-polishing resin, rosin, graphene-modified organic boron antifouling agent, copper pyrithione, zinc oxide, titanium oxide, iron oxide, organic bentonite, talcum powder and xylene are fully mixed and sand-milled, and the particle size is less than 50 μm and then filtered to obtain a marine antifouling coating.

[0057] The prepared marine antifouling coating was subjected to a shallow sea immersion test. After 18 months, only part of the test plate surface effective area had one obvious marine organism (barnacle or lime worm). It can be seen that the prepared marine antifouling coating has effective antifouling performance.

[0058] Example 2

[0059] Preparation of graphene-modified organic boron antifouling agent:

[0060] S1: Add 300 mL of xylene, 1 part by weight of graphene oxide and 1 part by weight of pyridine triphenyl boron into a 500 mL flask, stir and heat to 50°C to react; after reacting for 2 hours, take 5 mL of the reaction solution and centrifuge to obtain a precipitate, and stop the reaction when the precipitate does not show stratification to obtain a reaction solution; wherein the acid value of the graphene oxide is (500-600) mgKOH / g;

[0061] S2: The reaction solution is filtered and dried to obtain a graphene-modified organic boron antifouling agent.

[0062] Preparation of marine antifouling coatings:

[0063] Weigh 100 parts of zinc acrylate self-polishing resin, 150 parts of rosin, 120 parts of graphene-modified organic boron antifouling agent, 50 parts of copper pyrithione, 30 parts of zinc oxide, 5 parts of titanium oxide, 5 parts of iron oxide, 5 parts of organic bentonite, 15 parts of talc and 250 parts of xylene respectively;

[0064] Zinc acrylate self-polishing resin, rosin, graphene-modified organic boron antifouling agent, copper pyrithione, zinc oxide, titanium oxide, iron oxide, organic bentonite, talcum powder and xylene are fully mixed and sand-milled, and the particle size is less than 50 μm and then filtered to obtain a marine antifouling coating.

[0065] The prepared marine antifouling coating was subjected to a shallow sea immersion test. After 18 months, there was no obvious marine organism attachment within the effective area of ​​the test plate surface, indicating that the prepared marine antifouling coating has effective antifouling performance.

[0066] Example 3

[0067] Preparation of graphene-modified organic boron antifouling agent:

[0068] S1: Add 300 mL of xylene, 1 part by weight of graphene oxide and 1 part by weight of pyridine triphenyl boron into a 500 mL flask, stir and heat to 60°C to react; after reacting for 2 hours, take 5 mL of the reaction solution and centrifuge to obtain a precipitate, and stop the reaction when the precipitate does not show stratification to obtain a reaction solution; wherein the acid value of the graphene oxide is (500-600) mgKOH / g;

[0069] S2: The reaction solution is filtered and dried to obtain a graphene-modified organic boron antifouling agent.

[0070] Preparation of marine antifouling coatings:

[0071] Weigh 100 parts of zinc acrylate self-polishing resin, 100 parts of rosin, 120 parts of graphene-modified organic boron antifouling agent, 60 parts of copper pyrithione, 20 parts of zinc oxide, 10 parts of titanium oxide, 10 parts of iron oxide, 5 parts of organic bentonite, 10 parts of talc and 200 parts of xylene respectively;

[0072] Zinc acrylate self-polishing resin, rosin, graphene-modified organic boron antifouling agent, copper pyrithione, zinc oxide, titanium oxide, iron oxide, organic bentonite, talcum powder and xylene are fully mixed and sand-milled, and the particle size is less than 50 μm and then filtered to obtain a marine antifouling coating.

[0073] The prepared marine antifouling coating was subjected to a shallow sea immersion test. After 18 months, only part of the test plate surface effective area had one obvious marine organism (barnacle or lime worm). It can be seen that the prepared marine antifouling coating has effective antifouling performance.

[0074] Example 4

[0075] Preparation of graphene-modified organic boron antifouling agent:

[0076] S1: Add 300 mL of xylene, 1 part by weight of graphene oxide and 3 parts by weight of pyridine triphenyl boron into a 500 mL flask, stir and heat to 80°C to react; after reacting for 2 hours, take 5 mL of the solution and centrifuge to obtain a precipitate, and stop the reaction when the precipitate does not show stratification to obtain a reaction solution; wherein the acid value of the graphene oxide is (500-600) mgKOH / g;

[0077] S2: The reaction solution is filtered and dried to obtain a graphene-modified organic boron antifouling agent.

[0078] Preparation of marine antifouling coatings:

[0079] Weigh 100 parts of zinc acrylate self-polishing resin, 50 parts of rosin, 80 parts of graphene-modified organic boron antifouling agent, 50 parts of copper pyrithione, 50 parts of zinc oxide, 15 parts of titanium oxide, 15 parts of iron oxide, 10 parts of organic bentonite, 15 parts of talc and 150 parts of xylene respectively;

[0080] Zinc acrylate self-polishing resin, rosin, graphene-modified organic boron antifouling agent, copper pyrithione, zinc oxide, titanium oxide, iron oxide, organic bentonite, talcum powder and xylene are fully mixed and sand-milled, and the particle size is less than 50 μm and then filtered to obtain a marine antifouling coating.

[0081] The prepared marine antifouling coating was subjected to a shallow sea immersion test. After 18 months, there was no obvious marine organism attachment within the effective area of ​​the test plate surface, indicating that the prepared marine antifouling coating has effective antifouling performance.

[0082] Example 5

[0083] Preparation of graphene-modified organic boron antifouling agent:

[0084] S1: Add 300 mL of xylene, 1 part by weight of graphene oxide and 2 parts by weight of pyridine triphenyl boron into a 500 mL flask, stir and heat to 70°C to react; after reacting for 2 hours, take 5 mL of the solution and centrifuge to obtain a precipitate, and stop the reaction when the precipitate does not show stratification to obtain a reaction solution; wherein the acid value of the graphene oxide is (500-600) mgKOH / g;

[0085] S2: The reaction solution is filtered and dried to obtain a graphene-modified organic boron antifouling agent.

[0086] Preparation of marine antifouling coatings:

[0087] Weigh 100 parts of zinc acrylate self-polishing resin, 80 parts of rosin, 100 parts of graphene-modified organic boron antifouling agent, 70 parts of copper pyrithione, 40 parts of zinc oxide, 10 parts of titanium oxide, 10 parts of iron oxide, 5 parts of organic bentonite, 5 parts of talc and 180 parts of xylene respectively;

[0088] Zinc acrylate self-polishing resin, rosin, graphene-modified organic boron antifouling agent, copper pyrithione, zinc oxide, titanium oxide, iron oxide, organic bentonite, talcum powder and xylene are fully mixed and sand-milled, and the particle size is less than 50 μm and then filtered to obtain a marine antifouling coating.

[0089] The prepared marine antifouling coating was subjected to a shallow sea immersion test. After 18 months, there was no obvious marine organism attachment within the effective area of ​​the test plate surface, which shows that the prepared marine antifouling coating has effective antifouling performance.

[0090] Comparative Example 1

[0091] The graphene-modified organic boron antifouling agent is prepared according to the following process:

[0092] 300 mL of xylene, 1 part by weight of graphene oxide and 5 parts by weight of pyridine triphenyl boron were added to a 500 mL flask, and the mixture was stirred and heated to 90° C. to react; wherein the acid value of the graphene oxide was (500-600) mgKOH / g;

[0093] After a period of reaction, a small amount of the solution in the flask was taken for centrifugal separation. The precipitate was always separated into layers, and graphene oxide and pyridine triphenylborane could not react completely.

[0094] Comparative Example 2

[0095] Preparation of antifouling agent / graphene composite:

[0096] Graphene is oxidized to generate graphene oxide, and then Cu 2+ 、Zn 2+ The antifouling agent / graphene composite is covalently grafted onto the graphene surface, and pyridine triphenylborane is adsorbed on the graphene surface through hydrogen bonding and van der Waals forces to generate an antifouling agent / graphene composite with a high loading rate.

[0097] Weigh 100 parts of zinc acrylate self-polishing resin, 50 parts of rosin, 80 parts of antifouling agent / graphene composite, 80 parts of copper pyrithione, 50 parts of zinc oxide, 5 parts of titanium oxide, 5 parts of iron oxide, 15 parts of organic bentonite, 10 parts of talc and 150 parts of xylene respectively;

[0098] Zinc acrylate self-polishing resin, rosin, antifouling agent / graphene composite, copper pyrithione, zinc oxide, titanium oxide, iron oxide, organic bentonite, talcum powder and xylene are fully mixed and sand-ground, and the particle size is less than 50 μm and then filtered to obtain a marine antifouling coating.

[0099] The prepared marine antifouling coating was subjected to a shallow sea immersion test. After 18 months, a large area of ​​initial green algae had attached to the surface of the test board, and there was also obvious attachment of marine organisms.

[0100] From the data in Examples 1 to 4 and Comparative Example 2, it can be seen that in Examples 1 to 4, only part of the test plate surface effective area has one obvious marine organism (barnacle or limeworm), while the test plate surface in Comparative Example 2 has a large area of ​​initial green algae attached and obvious marine organisms attached, indicating that the graphene-modified organic boron antifouling agent prepared by the method disclosed in the present invention has a better antifouling effect.

[0101] The present invention is described in detail above in combination with specific implementation methods and exemplary examples. The above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments; the above description cannot be understood as limiting the present invention. Those skilled in the art understand that, without departing from the spirit and scope of the present invention, the technical solution of the present invention and its implementation methods may be subjected to a variety of equivalent substitutions, modifications or improvements, all of which fall within the scope of the present invention; the protection scope of the present invention shall be subject to the attached claims.

Claims

1. A marine antifouling coating, characterized in that: The following components are included by weight: 100 parts of zinc acrylate self-polishing resin; 50-150 parts of rosin; 80-120 parts of graphene-modified organic boron antifouling agent; 50-80 parts of copper pyrithione; 20-50 parts of zinc oxide; 5-15 parts of titanium oxide; 5-15 parts of iron oxide; 5-15 parts of organic bentonite; 5-15 parts of talcum powder; 150-250 parts of xylene; The graphene-modified organic boron antifouling agent is prepared by the following method: Xylene, graphene oxide and pyridine triphenyl boron are added into a reaction device for reaction to obtain a graphene-modified organic boron antifouling agent.

2. The marine antifouling coating according to claim 1, characterized in that: The number average molecular weight of the zinc acrylate self-polishing resin is 2000-3000.

3. The marine antifouling coating according to claim 2, characterized in that: The mass percentage content of Zn in the zinc acrylate self-polishing resin is 6% to 7%.

4. The marine antifouling paint according to claim 1, characterized in that: The graphene-modified organic boron antifouling agent is prepared by the following method: S1: adding xylene, graphene oxide and pyridine triphenylborane into a reaction device, stirring and heating to react; stopping the reaction until the precipitate obtained after centrifugal separation of the solution does not show stratification, and obtaining a reaction solution; S2: The reaction solution is filtered and dried to obtain a graphene-modified organic boron antifouling agent.

5. The marine antifouling paint according to claim 4, characterized in that: The amount of xylene used is 1 / 3 to 2 / 3 of the capacity of the reaction device.

6. The marine antifouling paint according to claim 4, characterized in that: The step S1 comprises: adding xylene, graphene oxide and pyridine triphenyl boron into a reaction device, stirring and heating to 50° C. to 90° C.

7. The marine antifouling paint according to claim 4, characterized in that: The mass ratio of the graphene oxide to pyridine triphenyl boron is 1:(1-3).

8. The marine antifouling paint according to claim 4, characterized in that: The acid value of the graphene oxide is 500-600 mgKOH / g.

9. A method for preparing a marine antifouling coating according to any one of claims 1 to 8, characterized in that: The following steps are involved: S10: weigh each component and set aside; S20: Fully mix and grind zinc acrylate self-polishing resin, rosin, graphene-modified organic boron antifouling agent, copper pyrithione, zinc oxide, titanium oxide, iron oxide, organic bentonite, talcum powder and xylene, filter and obtain the marine antifouling coating after the particle size is less than 50 μm.

Citation Information

Patent Citations

  • Marine antifouling paint

    CN110982359A

  • Environment-friendly graphene-based aqueous antifouling paint and preparation method thereof

    CN111378343A

  • Underwater antifouling coating containing triphenyl(alkylenediamine)boron

    JP2000143672A

  • Porous 3-dimensional structure in which holey graphene oxides are interlayer-linked and preparation thereof

    KR1020150112225A

  • Polypyrrole-graphene / polyurethane antifouling coating as well as preparation method and application thereof

    US20230126942A1