Antifouling electric porcelain insulator and preparation method thereof
By using a blend of fluorosilicone-modified epoxy resin and silicone rubber on the surface of the insulator to form a dense coating, the problem of existing anti-pollution flashover coatings being susceptible to high temperatures and weathering during outdoor use is solved, thus improving the insulator's high anti-pollution performance and weather resistance.
Patent Information
- Application Number
- CN202411167716.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-08
AI Technical Summary
Existing anti-pollution flashover coatings are susceptible to high temperatures and weathering when used outdoors, leading to a decline in anti-pollution performance and an inability to effectively prevent leakage current from the surface of insulators.
Fluorosilicone modified epoxy resin is blended with silicone rubber, and by introducing fluorine and inorganic fillers, a dense coating is formed, which improves the anti-fouling performance and weather resistance of the coating and enhances the overall performance of the insulator.
It significantly improves the hydrophobicity and oleophobicity of the coating, enhances the weather resistance and overall performance of the insulator, reduces surface charge accumulation, optimizes the electric field distribution, and prevents surface flashover.
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of insulators, and in particular to an anti-pollution electric porcelain insulator and a preparation method thereof. Background Art
[0002] Post insulators are very important electrical equipment in the power system. Their quality is directly related to whether the power system can operate safely, and is particularly important for high-voltage transmission lines. Pollutants on the surface of insulators are the main cause of insulator flashovers. Flashover accidents usually manifest as continuous flashover accidents, which not only cause equipment damage, but may also cause major safety accidents such as fires and explosions. Therefore, anti-flashover treatment of the insulator surface is a key measure to ensure the safe and stable operation of the power system.
[0003] At present, the commonly used anti-pollution flashover methods include cleaning, applying anti-pollution flashover paint and hanging porcelain sleeves. Insulators coated with room temperature vulcanized anti-pollution flashover paint can give substation equipment strong hydrophobicity, hydrophobic migration and hydrophobic recovery properties. Even if its surface is covered with solid particles, it still maintains hydrophobicity so that a continuous water film cannot be formed on its surface, thereby preventing leakage current from being generated on its surface and ensuring that no flashover voltage is generated. The anti-pollution flashover coating in related technologies is usually a method of coating silicone rubber on the surface of the insulator, but silicone rubber is an elastic material and is easily affected by high temperature and weathering when used outdoors for a long time, which reduces the anti-pollution performance.
[0004] Application Contents
[0005] The present application has been made in view of the above-mentioned problems, and an object of the present application is to provide a pollution-proof electric porcelain insulator having a large contact angle and excellent pollution-proof performance.
[0006] Specifically, the first aspect of the present application provides an anti-fouling electric porcelain insulator, including an insulator body and a coating;
[0007] The coating comprises the following preparation materials:
[0008] Silicone rubber, tridecafluorooctyltrimethoxysilane, fluorine-silicon modified epoxy resin, filler;
[0009] Fluorosilicone modified epoxy resin includes the following preparation raw materials:
[0010] Epoxy resin, heptadecafluorodecyltrimethoxysilane, p-aminophenyltrimethoxysilane, and silica.
[0011] According to one of the technical solutions of this application, at least the following beneficial effects are achieved:
[0012] The present application adds fluorine-silicon modified epoxy resin to silicone rubber blend as a matrix material, thereby introducing fluorine element into the coating, thereby improving the antifouling performance, stability and weather resistance of the coating.
[0013] The present invention uses aminosilicone and fluorosilane to react to generate fluorosilicone resin; uses fluorosilicone resin as a modifier to modify epoxy resin, and the amino groups in the fluorosilicone resin react with the epoxy groups in the epoxy resin to undergo ring-opening polymerization to obtain fluorosilicone epoxy resin.
[0014] Because the main chain of fluorosilicone resin contains inorganic Si-O bonds with high bond energy, it has the high temperature stability and high hardness of inorganic materials; the short chain of fluorinated silicone is firmly wedged into the epoxy cross-linking network through chemical bonds, which increases the density of the coating. At the same time, the generated Si-O bonds have large bond energy and chemically bond with the OH bonds on the surface of the substrate. C-Si can rotate, which improves the tensile strength and adhesion of the fluorosilicone modified epoxy resin to varying degrees; after the introduction of low surface energy fluorocarbon bonds and silicon-oxygen bonds into the epoxy resin, the coating becomes water-repellent and oil-repellent, which can significantly improve the weather resistance of the coating.
[0015] The use of inorganic fillers can greatly increase the volume resistivity of insulators, reduce surface charge accumulation, optimize electric field distribution, avoid surface flashover, and at the same time improve the insulation, mechanical and thermal properties of insulators.
[0016] Silicon dioxide has strong hardness and good corrosion resistance, good high temperature stability, good heat resistance, high strength, and excellent wear resistance. Using silicon dioxide to modify epoxy resin can effectively improve the breakdown strength of the coating, toughen the epoxy resin, reduce its sensitivity to cracks, increase dimensional stability, reduce the tendency of stress cracking, and enhance its pressure resistance and corrosion resistance.
[0017] According to some embodiments of the present application, the filler includes alumina, titanium dioxide and silicon dioxide.
[0018] According to some embodiments of the present application, the coating includes the following preparation raw materials in parts by weight:
[0019] 20 parts of silicone rubber, 4 to 6 parts of tridecafluorooctyltrimethoxysilane, 20 to 40 parts of fluorine silicon modified epoxy resin, 2 to 5 parts of aluminum oxide, 2 to 5 parts of titanium dioxide and 4 to 10 parts of silicon dioxide.
[0020] According to some embodiments of the present application, the raw materials for preparing the coating further include a catalyst, a dispersant and a solvent.
[0021] According to some embodiments of the present application, the solvent includes propylene glycol methyl ether acetate.
[0022] Silicone rubber and fluorosilicone resin modified epoxy resin have poor compatibility. The present application uses propylene glycol methyl ether acetate as a solvent to improve the compatibility between the two.
[0023] According to some embodiments of the present application, the catalyst is hydroxymethyldiethyltriamine.
[0024] According to some embodiments of the present application, the dispersant includes polyethylene glycol.
[0025] According to some embodiments of the present application, the coating includes the following preparation raw materials in parts by weight:
[0026] 20 parts of silicone rubber, 4 to 6 parts of tridecafluorooctyltrimethoxysilane, 20 to 40 parts of fluorosilicone modified epoxy resin, 2 to 5 parts of aluminum oxide, 2 to 5 parts of titanium dioxide, 4 to 10 parts of silicon dioxide, 0.1 to 1 part of catalyst, 0.1 to 1 part of dispersant and 30 to 50 parts of solvent.
[0027] According to some embodiments of the present application, the fluorine-silicon modified epoxy resin includes the following preparation raw materials in parts by weight:
[0028] 100 parts of epoxy resin, 10 to 20 parts of heptadecafluorodecyltrimethoxysilane, 5 to 10 parts of p-aminophenyltrimethoxysilane and 2 to 3 parts of silicon dioxide.
[0029] According to some embodiments of the present application, the raw materials for preparing the fluorine-silicon modified epoxy resin further include a solvent, an acid and a base.
[0030] According to some embodiments of the present application, the thickness of the coating is 0.3 mm to 0.5 mm.
[0031] According to some embodiments of the present application, the insulator body is a porcelain insulator.
[0032] According to some embodiments of the present application, the porcelain insulator includes the following raw materials in parts by weight:
[0033] Alumina 20%-30%, feldspar 15%-25%, ball clay 20%-25%, clay 20%-25% and strontium carbonate 3%-5%.
[0034] The second aspect of the present application provides a method for preparing the insulator according to the first aspect of the present application, comprising the following steps:
[0035] The coating is applied on the surface of the insulator body.
[0036] According to some embodiments of the present application, the method for preparing the fluorine-silicon modified epoxy resin comprises the following steps:
[0037] S1, mixing heptadecafluorodecyltrimethoxysilane, p-aminophenyltrimethoxysilane, an acid and a solvent and reacting them to obtain a fluorosilicone resin;
[0038] S2, mixing fluorosilicone resin, alkali, epoxy resin and solvent and reacting them.
[0039] According to some embodiments of the present application, the pH of the reaction in step S1 is 4-5.
[0040] According to some embodiments of the present application, the temperature of the reaction in step S1 is 60°C to 70°C.
[0041] According to some embodiments of the present application, the reaction time in step S1 is 1 h to 2 h.
[0042] According to some embodiments of the present application, the temperature of the reaction in step S2 is 120°C to 140°C.
[0043] According to some embodiments of the present application, the reaction time in step S2 is 1 h to 2 h.
[0044] According to some embodiments of the present application, the solvent in step S1 includes water and ethanol.
[0045] According to some embodiments of the present application, the solvent in step S2 includes isobutanol and butyl acetate. DETAILED DESCRIPTION
[0046] In order to make the purpose, technical solutions and advantages of the present application clearer, the present application is described and illustrated below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not intended to limit the present application. Based on the embodiments provided in the present application, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present application.
[0047] Obviously, the following descriptions are only some examples or embodiments of the present application. For ordinary technicians in this field, the present application can also be applied to other similar scenarios without creative work. In addition, it can also be understood that although the efforts made in this development process may be complicated and lengthy, for ordinary technicians in the field related to the content disclosed in this application, some changes in design, manufacturing or production based on the technical content disclosed in this application are just conventional technical means, and should not be understood as insufficient content disclosed in this application.
[0048] However, unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repeated descriptions of substantially the same structures may be omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate understanding by those skilled in the art. In addition, the following description is provided for those skilled in the art to fully understand the present application and is not intended to limit the subject matter described in the claims.
[0049] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0050] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0051] "Scope" disclosed in the present application is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values 1 and 2 are listed, and if the maximum range values 3, 4 and 5 are listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0052] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0053] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0054] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0055] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or included, or may only include or include the listed components.
[0056] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0057] The preparation method of the insulator body in the embodiments and comparative examples of the present application comprises the following steps:
[0058] The raw materials of the blank are as follows: 25% alumina, 25% feldspar, 20% ball clay, 25% clay and 5% SrCO3, wherein the particle size of the clay granules is 40 mesh;
[0059] S1. Sand-grinding the blank raw material to obtain blank particles, the diameter of the blank particles can reach 3μm to 5μm;
[0060] S2, loading the above-mentioned blank particles into a ball mill, and ball milling them at a mass percentage of blank: water: ball stone = (1:1:2), and ball milling for 12 hours;
[0061] S3, the ball mill is screened four times and iron removed six times, the fineness reaches below 40 μm, 90% of the iron impurities and coarse particles larger than 40 μm in the raw material are removed, and the mud is obtained;
[0062] S4, after the clay is made into clay segments, it is dried (drying temperature is 110°C, time is 42h), glazed and sintered (sintering temperature is 1250°C);
[0063] During the glazing process, the specific gravity, viscosity and thickness of the glaze slurry are 1.38-1.48 g / cm 3 , 0.15~0.30Pa·S and 0.3mm±0.05mm.
[0064] Example 1
[0065] This embodiment is an anti-fouling electric porcelain insulator, comprising an insulator body and a coating (thickness of 0.4 mm);
[0066] The coating comprises the following raw materials in parts by weight:
[0067] 20 parts of silicone rubber (107# room temperature vulcanized silicone rubber), 6 parts of tridecafluorooctyltrimethoxysilane, 40 parts of fluorosilicone modified epoxy resin, 4 parts of aluminum oxide (D50 is 100nm), 3 parts of titanium dioxide (D50 is 200nm), 8 parts of silicon dioxide (D50 is 50nm), 0.5 parts of catalyst (hydroxymethyldiethyltriamine), 0.5 parts of dispersant (polyethylene glycol 400) and 30 parts of solvent (propylene glycol methyl ether acetate).
[0068] The fluorine-silicon modified epoxy resin includes the following raw materials in parts by weight:
[0069] 100 parts of epoxy resin, 20 parts of heptadecafluorodecyltrimethoxysilane, 10 parts of p-aminophenyltrimethoxysilane and 3 parts of silicon dioxide.
[0070] The preparation method of fluorine-silicon modified epoxy resin consists of the following steps:
[0071] S1. Heptadecafluorodecyltrimethoxysilane, p-aminophenyltrimethoxysilane, an acid (hydrochloric acid with a mass fraction of 30%) and a solvent (ethanol aqueous solution with a volume fraction of 70%, and a volume mass ratio of ethanol aqueous solution to heptadecafluorodecyltrimethoxysilane of 1 g:1 mL) are mixed and reacted (the pH of the reaction is 4, the temperature is 65° C., and the time is 2 h). After the reaction is completed, the fluorosilicone resin is obtained by distillation under reduced pressure;
[0072] S2. Mix fluorosilicone resin, alkali (sodium hydroxide, the mass ratio of sodium hydroxide to epoxy resin is 0.1:1), epoxy resin (E51), silica and solvent (isobutyl alcohol and butyl acetate are mixed in a volume ratio of 1:1, and the mass volume ratio of epoxy resin to solvent is 1g:2mL) and react (the reaction temperature is 140°C and the reaction time is 1h). After the reaction is completed, distill under reduced pressure.
[0073] The method for preparing an insulator in this embodiment includes the following steps:
[0074] The raw materials for preparing the coating are mixed and then sprayed on the surface of the insulator body, and naturally cured at 25° C. to form a coating on the surface of the insulator body.
[0075] The mixing method of the raw materials for preparing the coating in this embodiment is as follows:
[0076] The method for preparing the anti-pollution flashover spray composite material for external insulation of power transmission lines in this embodiment comprises the following steps:
[0077] S1, mixing silicone rubber, fluorosilicone resin-modified epoxy resin, tridecafluorooctyltrimethoxysilane and solvent, and stirring at 1500 rpm for 2 hours to obtain a first mixture;
[0078] S2, adding aluminum oxide, titanium dioxide and silicon dioxide to the first mixture, stirring at 10000 rpm for 2 hours after the addition, to obtain a second mixture;
[0079] S3. Add dispersant to the second mixture, mix at 1500 rpm for 2 hours, then add catalyst, and mix at 1500 rpm for 2 hours.
[0080] Example 2
[0081] This embodiment is an anti-fouling electric porcelain insulator, comprising an insulator body and a coating (thickness of 0.4 mm);
[0082] The coating comprises the following raw materials in parts by weight:
[0083] 20 parts of silicone rubber (107# room temperature vulcanized silicone rubber), 5 parts of tridecafluorooctyltrimethoxysilane, 30 parts of fluorosilicone modified epoxy resin, 4 parts of aluminum oxide (D50 is 100nm), 3 parts of titanium dioxide (D50 is 200nm), 5 parts of silicon dioxide (D50 is 50nm), 0.5 parts of catalyst (hydroxymethyldiethyltriamine), 0.5 parts of dispersant (polyethylene glycol 400) and 30 parts of solvent (propylene glycol methyl ether acetate).
[0084] The fluorine-silicon modified epoxy resin includes the following raw materials in parts by weight:
[0085] 100 parts of epoxy resin, 14 parts of heptadecafluorodecyltrimethoxysilane, 6 parts of p-aminophenyltrimethoxysilane and 2.4 parts of silicon dioxide.
[0086] The preparation method of the fluorine-silicon modified epoxy resin and the insulator in this embodiment is carried out with reference to that in Embodiment 1.
[0087] Example 3
[0088] This embodiment is an anti-fouling electric porcelain insulator, comprising an insulator body and a coating (thickness of 0.4 mm);
[0089] The coating comprises the following raw materials in parts by weight:
[0090] 20 parts of silicone rubber (107# room temperature vulcanized silicone rubber), 5 parts of tridecafluorooctyltrimethoxysilane, 25 parts of fluorosilicone modified epoxy resin, 3 parts of aluminum oxide (D50 is 100nm), 5 parts of titanium dioxide (D50 is 200nm), 6 parts of silicon dioxide (D50 is 50nm), 0.5 parts of catalyst (hydroxymethyldiethyltriamine), 0.5 parts of dispersant (polyethylene glycol 400) and 30 parts of solvent (propylene glycol methyl ether acetate).
[0091] The fluorine-silicon modified epoxy resin includes the following raw materials in parts by weight:
[0092] 100 parts of epoxy resin, 13 parts of heptadecafluorodecyltrimethoxysilane, 5 parts of p-aminophenyltrimethoxysilane and 2 parts of silicon dioxide.
[0093] The preparation method of the fluorine-silicon modified epoxy resin and the insulator in this embodiment is carried out with reference to that in Embodiment 1.
[0094] Example 4
[0095] This embodiment is an anti-fouling electric porcelain insulator, comprising an insulator body and a coating (thickness of 0.4 mm);
[0096] The coating comprises the following raw materials in parts by weight:
[0097] 20 parts of silicone rubber (107# room temperature vulcanized silicone rubber), 4 parts of tridecafluorooctyltrimethoxysilane, 20 parts of fluorosilicone modified epoxy resin, 5 parts of aluminum oxide (D50 is 100nm), 5 parts of titanium dioxide (D50 is 200nm), 10 parts of silicon dioxide (D50 is 50nm), 0.5 parts of catalyst (hydroxymethyldiethyltriamine), 0.5 parts of dispersant (polyethylene glycol 400) and 30 parts of solvent (propylene glycol methyl ether acetate).
[0098] The fluorine-silicon modified epoxy resin includes the following raw materials in parts by weight:
[0099] 100 parts of epoxy resin, 12 parts of heptadecafluorodecyltrimethoxysilane, 8 parts of p-aminophenyltrimethoxysilane and 3 parts of silicon dioxide.
[0100] The preparation method of the fluorine-silicon modified epoxy resin and the insulator in this embodiment is carried out with reference to that in Embodiment 1.
[0101] Example 5
[0102] This embodiment is an anti-fouling electric porcelain insulator, comprising an insulator body and a coating (thickness of 0.4 mm);
[0103] The coating comprises the following raw materials in parts by weight:
[0104] 20 parts of silicone rubber (107# room temperature vulcanized silicone rubber), 4 parts of tridecafluorooctyltrimethoxysilane, 20 parts of fluorosilicone modified epoxy resin, 2 parts of aluminum oxide (D50 is 100nm), 2 parts of titanium dioxide (D50 is 200nm), 4 parts of silicon dioxide (D50 is 50nm), 0.5 parts of catalyst (hydroxymethyldiethyltriamine), 0.5 parts of dispersant (polyethylene glycol 400) and 30 parts of solvent (propylene glycol methyl ether acetate).
[0105] The fluorine-silicon modified epoxy resin includes the following raw materials in parts by weight:
[0106] 100 parts of epoxy resin, 10 parts of heptadecafluorodecyltrimethoxysilane, 5 parts of p-aminophenyltrimethoxysilane and 2 parts of silicon dioxide.
[0107] The preparation method of the fluorine-silicon modified epoxy resin and the insulator in this embodiment is carried out with reference to that in Embodiment 1.
[0108] Comparative Example 1
[0109] This comparative example is an anti-pollution insulator, which differs from Example 5 in that:
[0110] The fluorine-silicon modified epoxy resin includes the following raw materials in parts by weight:
[0111] 100 parts of epoxy resin, 10 parts of heptadecafluorodecyltrimethoxysilane, and 5 parts of p-aminophenyltrimethoxysilane.
[0112] The preparation method of fluorine-silicon modified epoxy resin consists of the following steps:
[0113] S1. Heptadecafluorodecyltrimethoxysilane, p-aminophenyltrimethoxysilane, an acid (hydrochloric acid with a mass fraction of 30%) and a solvent (ethanol aqueous solution with a volume fraction of 70%, and a volume mass ratio of ethanol aqueous solution to heptadecafluorodecyltrimethoxysilane of 1 g:1 mL) are mixed and reacted (the pH of the reaction is 4, the temperature is 65° C., and the time is 2 h). After the reaction is completed, the fluorosilicone resin is obtained by distillation under reduced pressure;
[0114] S2. Mix fluorosilicone resin, alkali (sodium hydroxide, the mass ratio of sodium hydroxide to epoxy resin is 0.1:1), epoxy resin (E51) and solvent (isobutyl alcohol and butyl acetate are mixed in a volume ratio of 1:1, and the mass volume ratio of epoxy resin to solvent is 1g:2mL) and react (the reaction temperature is 140°C and the reaction time is 1h). After the reaction is completed, distill under reduced pressure.
[0115] Comparative Example 2
[0116] This comparative example is an anti-pollution insulator, which differs from Example 5 in that:
[0117] Replace fluorine-silicone modified epoxy resin with fluorine-modified epoxy resin.
[0118] The fluorine-modified epoxy resin includes the following raw materials in parts by weight:
[0119] 100 parts of epoxy resin, 10 parts of heptadecafluorodecyltrimethoxysilane and 2 parts of silicon dioxide.
[0120] The preparation method of fluorine-modified epoxy resin consists of the following steps:
[0121] Heptadecafluorodecyltrimethoxysilane, epoxy resin (E51), silica and solvent (isobutyl alcohol and butyl acetate are mixed in a volume ratio of 1:1, and the mass volume ratio of epoxy resin and solvent is 1g:2mL) are mixed (temperature is 140°C, time is 1h), and after mixing, the mixture is distilled under reduced pressure.
[0122] Comparative Example 3
[0123] This comparative example is an anti-pollution insulator, which differs from Example 5 in that:
[0124] Replace fluorine-silicon-modified epoxy resin with silicon-modified epoxy resin.
[0125] The silicon-modified epoxy resin comprises the following raw materials in parts by weight:
[0126] 100 parts of epoxy resin, 5 parts of p-aminophenyltrimethoxysilane and 2 parts of silicon dioxide.
[0127] The preparation method of silicon-modified epoxy resin consists of the following steps:
[0128] Para-aminophenyltrimethoxysilane, alkali (sodium hydroxide, the mass ratio of sodium hydroxide to epoxy resin is 0.1:1), epoxy resin (E51), silica and solvent (isobutyl alcohol and butyl acetate are mixed in a volume ratio of 1:1, and the mass volume ratio of epoxy resin to solvent is 1g:2mL) are mixed and reacted (the reaction temperature is 140°C and the reaction time is 1h), and then distilled under reduced pressure after the reaction is completed.
[0129] Comparative Example 4
[0130] This comparative example is an anti-pollution insulator, which differs from Example 5 in that:
[0131] Replace the fluorine-silicon modified epoxy resin with a silica-modified epoxy resin.
[0132] The silicon dioxide modified epoxy resin comprises the following raw materials in parts by weight:
[0133] 100 parts of epoxy resin and 2 parts of silica.
[0134] The preparation method of fluorine-silicon modified epoxy resin consists of the following steps:
[0135] Epoxy resin (E51), silica and solvent (isobutyl alcohol and butyl acetate are mixed in a volume ratio of 1:1, and the mass volume ratio of epoxy resin and solvent is 1g:2mL) are mixed (temperature is 140°C, time is 1h), and after mixing, they are distilled under reduced pressure.
[0136] Comparative Example 5
[0137] This comparative example is an anti-pollution insulator, which differs from Example 5 in that:
[0138] The fluorine-silicone modified epoxy resin was replaced with epoxy resin (E51).
[0139] The performance test results of the coatings in the examples and comparative examples of the present application are shown in Table 1, and the test methods are as follows:
[0140] The raw materials for preparing the coatings in the examples and comparative examples were mixed (the mixing method was carried out in accordance with that in Example 1) and then coated on a glass sheet. After being completely cured at 25° C., the contact angle was tested.
[0141] Contact angle: Use a contact angle tester.
[0142] Volume resistivity: Tested in accordance with standard DLT 627.
[0143] Table 1
[0144] - <![CDATA[Volume resistivity (*10 15 Ω·m)]]> Contact angle (°) Example 1 1.52 137.3 Example 2 1.47 136.1 Example 3 1.46 133.2 Example 4 1.41 131.9 Example 5 1.38 130.5 Comparative Example 1 1.28 124.3 Comparative Example 2 1.21 121.6 Comparative Example 3 1.12 117.3 Comparative Example 4 1.05 115.2 Comparative Example 5 0.93 107.0
[0145] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.
Claims
1. A pollution-proof electric porcelain insulator, characterized in that: Including insulator body and coating; The coating comprises the following preparation materials: Silicone rubber, tridecafluorooctyltrimethoxysilane, fluorine-silicon modified epoxy resin, filler; Fluorosilicone modified epoxy resin includes the following preparation raw materials: Epoxy resin, heptadecafluorodecyltrimethoxysilane, p-aminophenyltrimethoxysilane, and silica.
2. The insulator according to claim 1, characterized in that: The filler includes alumina, titanium dioxide and silicon dioxide; And / or, the coating comprises the following preparation raw materials in parts by weight: 20 parts of silicone rubber, 4 to 6 parts of tridecafluorooctyltrimethoxysilane, 20 to 40 parts of fluorine-silicon modified epoxy resin, 2 to 5 parts of aluminum oxide, 2 to 5 parts of titanium dioxide and 4 to 10 parts of silicon dioxide; And / or, the raw materials for preparing the coating further include a catalyst, a dispersant and a solvent; and / or, the solvent comprises propylene glycol methyl ether acetate; and / or, the dispersant comprises polyethylene glycol; And / or, the catalyst is hydroxymethyldiethyltriamine; And / or, the coating comprises the following preparation raw materials in parts by weight: 20 parts of silicone rubber, 4 to 6 parts of tridecafluorooctyltrimethoxysilane, 20 to 40 parts of fluorosilicone modified epoxy resin, 2 to 5 parts of aluminum oxide, 2 to 5 parts of titanium dioxide, 4 to 10 parts of silicon dioxide, 0.1 to 1 part of catalyst, 0.1 to 1 part of dispersant and 30 to 50 parts of solvent.
3. The insulator according to claim 1, characterized in that: The fluorine-silicon modified epoxy resin comprises the following raw materials in parts by weight: 100 parts of epoxy resin, 10 to 20 parts of heptadecafluorodecyltrimethoxysilane, 5 to 10 parts of p-aminophenyltrimethoxysilane and 2 to 3 parts of silicon dioxide; And / or, the raw materials for preparing the fluorine-silicon modified epoxy resin further include a solvent, an acid and a base.
4. The insulator according to claim 1, characterized in that: The thickness of the coating is 0.3 mm to 0.5 mm.
5. The insulator according to claim 1, characterized in that: The insulator body is a porcelain insulator; And / or, the porcelain insulator comprises the following raw materials in parts by weight: Alumina 20%-30%, feldspar 15%-25%, ball clay 20%-25%, clay 20%-25% and strontium carbonate 3%-5%.
6. A method for preparing an insulator according to any one of claims 1 to 5, characterized in that: The following steps are involved: The coating is applied on the surface of the insulator body.
7. The preparation method according to claim 6, characterized in that: The preparation method of the fluorine-silicon modified epoxy resin comprises the following steps: S1, mixing heptadecafluorodecyltrimethoxysilane, p-aminophenyltrimethoxysilane, an acid and a solvent and reacting them to obtain a fluorosilicone resin; S2, mixing fluorosilicone resin, alkali, epoxy resin and solvent and reacting them.
8. The preparation method according to claim 7, characterized in that: The pH of the reaction in step S1 is 4-5; And / or, the reaction temperature in step S1 is 60°C to 70°C; And / or, the reaction time in step S1 is 1 h to 2 h.
9. The preparation method according to claim 7, characterized in that: The reaction temperature in step S2 is 120°C to 140°C; And / or, the reaction time in step S2 is 1 h to 2 h.
10. The preparation method according to claim 7, characterized in that: The solvent in step S1 includes water and ethanol; And / or, the solvent in step S2 includes isobutanol and butyl acetate.
Citation Information
Patent Citations
Novel external insulating anti-pollution flashover spraying composite material of electric transmission line
CN107663416A
Preparation method of epoxy resin for motor insulation based on nano modification
CN114106513A