Anti-aging and anti-tearing safety airbag coating and preparation method thereof

Through the cross-linking reaction of vinyl silicone oil and phenyl vinyl silicone oil and the combination of vinyl fluorine-containing silicone oil, the problem of aging and deterioration of the airbag coating after gunpowder explosion is solved, and the coating resistance to tear and resistance is improved High temperature performance ensures the stability and safety of the airbag.

CN118909543AActive Publication Date: 2024-11-08JIANGSU ZHIXIN NEW MATERIALS CO LTD

Patent Information

Application Number
CN202411136317.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-08
Estimated Expiration
2044-08-19

AI Technical Summary

Technical Problem

The existing airbag coating materials age and deteriorate at the high temperatures caused by gunpowder explosion, resulting in reduced airbag strength, which may lead to tearing and explosion, causing serious harm.

Method used

The chemical structure is formed by cross-linking reaction of vinyl silicone oil and phenyl vinyl silicone oil, and the combination of vinyl fluoro-containing silicone oil is used to improve the aging resistance, water resistance, oil resistance and high temperature resistance of the coating, and through silicone chain extenders Optimize cross-linking reaction with the catalyst to enhance the mechanical properties and adhesion of the coating.

Benefits of technology

It significantly improves the coating's tear resistance, wear resistance, heat resistance and service life, ensuring that the airbag maintains stability and safety in high temperature environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004999531400000091
    Figure BDA0004999531400000091
  • Figure BDA0004999531400000101
    Figure BDA0004999531400000101
Patent Text Reader

Abstract

The invention relates to an automobile safety air bag coating material, in particular to an anti-aging and anti-tearing safety air bag coating and a preparation method thereof. The anti-aging and anti-tearing airbag coating comprises a component A and a component B. The component A comprises the following components in parts by weight: 65-85 parts of vinyl silicone oil, 12-15 parts of an organic silicon chain extender, 3-5.5 parts of an organic silicon cross-linking agent, 0.05-0.1 part of an inhibitor and 2.5-3 parts of a silane coupling agent. And the component B comprises the following components in parts by weight: 40-80 parts of vinyl fluorine-containing silicone oil, 0.1-0.7 part of a catalyst, 1.5-3 parts of a tackifier and 1-3 parts of an anti-aging agent DW. According to the anti-aging and anti-tearing safety air bag coating, the problem that an existing safety air bag is poor in tearing resistance and aging resistance is solved, namely, the situation that an air bag is aged and degraded, the strength is reduced, the air bag is torn, seam holes are torn and even burst during use, and a driver or passengers are seriously damaged is prevented.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to a coating material for an automobile airbag, and more specifically, to an anti-aging and tearing airbag coating and a preparation method thereof. Background Art

[0002] In recent years, with the expansion of the automobile market, automobiles have become an indispensable means of transportation. As a result, the safety of automobile use has attracted more and more attention. Airbags are important components of passive safety systems that are widely used in automobiles. They can effectively reduce the deceleration impact and secondary collision force that occupants suffer in a collision. In a very short time, an elastic air cushion is formed in front of or on the side of the driver or passenger, and the pressure is released and contracted in time to absorb the impact energy, thereby effectively protecting the human head and chest. It is an important and effective protection measure for drivers or passengers in car collisions. The types, installation rates and safety of airbags are also receiving more and more attention.

[0003] In the existing airbags, the gunpowder of the gas generator explodes, and the airbag is deployed only 0.003ms later, and the airbag shrinks 0.2ms later. The maximum temperature of the gunpowder explosion can reach 2000℃. The existing airbag coating materials have excellent properties such as moisture resistance, fire resistance, insulation and sealing. With the development of the automobile industry, the research and development of new coating materials with excellent performance is an important issue for our researchers, that is, to prevent the hot gas generated by the generator from escaping through the airbag coating, causing the airbag to age and deteriorate, and the strength to decrease, which eventually leads to the tearing of the airbag, the tearing of the seam hole, and even the bursting of the airbag, causing serious harm to the driver or passengers. Summary of the invention

[0004] In view of the problem that the existing airbag coating has poor tear resistance and aging resistance, the present application provides an anti-aging and tear-resistant airbag coating and a preparation method thereof.

[0005] In the first aspect, the present application provides an anti-aging and tear-resistant airbag coating, which adopts the following technical solution: The invention comprises component A and component B, wherein component A comprises the following components in parts by weight: 65-85 parts of vinyl silicone oil, 12-15 parts of organosilicon chain extender, 3-5.5 parts of organosilicon crosslinker, 0.05-0.1 parts of inhibitor and 2.5-3 parts of silane coupling agent; component B comprises the following components in parts by weight: 40-80 parts of vinyl fluorine-containing silicone oil, 0.1-0.7 parts of catalyst, 1.5-3 parts of tackifier and 1-3 parts of antioxidant DW; the vinyl silicone oil of component A comprises vinyl-terminated polydimethylsiloxane and phenyl vinyl silicone oil.

[0006] By adopting the above technical scheme, a cross-linking framework is provided by reacting vinyl-terminated polydimethylsiloxane with phenyl vinyl silicone oil and hydrogen-containing silicone oil. The shielding effect of phenyl on the surrounding groups improves the chemical stability of the resin to a certain extent. After the vinyl and hydrogen-containing groups form cross-linking and curing, the conjugated electron effect between the phenyl groups further improves this effect, reduces the chemical activity of the resin polymer chain segment, improves the stability and strength of the coating, enhances the anti-aging performance of the material, and has excellent properties such as strong solvent resistance, water resistance, ablation resistance, and high temperature resistance. The inventors also added vinyl fluorinated silicone oil to the coating and found that the addition of phenyl vinyl silicone oil and vinyl fluorinated silicone oil significantly improved the aging resistance, water resistance and oil resistance of the coating, which may be due to , adding vinyl fluorinated silicone oil, the fluorinated groups in the vinyl fluorinated silicone oil are electron-withdrawing groups, and the vinyl group promotes the cross-linking density, so that the vinyl fluorinated silicone oil can generate intermolecular interaction forces with the above cross-linking framework, and be embedded or attached to the surface of the cross-linking network system; the fluorinated groups such as trifluoromethyl are dispersed in claws due to the steric hindrance effect between F and F, and the fluorinated groups and phenyl groups are in different silane side chains, so that some F atoms are exposed on the surface of the cross-linking system, and some are dispersed between the benzene rings, and are not shielded by the steric hindrance of the benzene rings, which can further enhance the shielding effect of the benzene rings, improve the aging resistance, and give full play to the hydrophobic and oleophobic properties of the vinyl fluorinated silicone oil and the anti-aging and stability of the phenyl group, and improve the cross-linking density of the system, and improve the tear resistance effect. In addition, the wear resistance, heat stability, oil resistance, corrosion resistance, etc. of the coating are also improved, and the service life of the coating is increased.

[0007] With the addition of organosilicon chain extenders, the long chains of the chain extenders can extend into the cross-linking structure, playing a role in strengthening the cross-linking points, thereby improving the overall stability and mechanical properties; using organosilicon cross-linkers and ensuring the smooth progress of the cross-linking reaction, improving the reaction efficiency, and effectively controlling the reaction process; the catalyst improves the cross-linking reaction efficiency between vinyl silicone oil and hydrogen-containing silicone oil such as organosilicon chain extenders, promotes the activation of hydrogen-containing silicone oil and double bonds, increases the number of strong interaction points between the silicone oil molecular chain and the catalytic metal center, and at the same time improves the stability of the catalyst metal after oxidation addition, prevents metal precipitation and inactivation, ensures the smooth progress of the cross-linking reaction, and then accelerates the combination of vinyl silicone oil and cross-linkers, chain extenders, etc., ensures that the product has good mechanical properties and stability, and enhances the material's tear resistance; by adding tackifiers and antioxidants, the compactness and anti-aging properties of the coating material are further improved. On the other hand, the addition of silane coupling agents can further improve the adhesion of the coating and prevent the coating from peeling off.

[0008] In a specific embodiment, the mass ratio of the vinyl-terminated polydimethylsiloxane to the phenyl vinyl silicone oil is (5-8):1.

[0009] By adopting the above technical scheme, a certain proportion of vinyl silicone oil is helpful to make the coating material wear resistance, and UV aging resistance test performance excellent, so that the coating material can maintain better stability in the face of a more complex external environment and is not easily destroyed, extending the service life of the material. The applicant found that the coating of phenyl vinyl silicone oil has better performance under the above ratio. When the phenyl content in the system is insufficient, the side chain structure is not tight enough, so that the adjacent phenyl force is small, the conjugated shielding effect is small, the overall stability and mechanical properties of the cross-linked framework structure are affected, and the aging resistance is poor; when the phenyl content in the system is too high, the side chain phenyl is too much, which is not conducive to the cross-linking reaction of the cross-linking system, resulting in a decrease in the strength of the cross-linking system, and poor aging resistance, and too much phenyl is easy to cause the shielding of the fluorinated group and reduce the hydrophobic and oleophobic properties. In addition, too many benzene rings also affect the flexibility of the coating.

[0010] In a specific embodiment, the vinyl fluorine-containing silicone oil of component B is vinyl-terminated fluorine silicone oil.

[0011] In a specific embodiment, the inhibitor is diallyl maleate; the adhesion promoter is isopropyl tri(dioctyl pyrophosphate) titanate; and the organosilicon crosslinker is polymethyl hydrogen siloxane.

[0012] In a specific embodiment, the silane coupling agent is KH560 and KH570 in a mass ratio of 1:2.

[0013] The organosilicon chain extender is hydrogen-terminated polydimethylsiloxane.

[0014] In a second aspect, the present application provides a method for preparing an anti-aging and tear-resistant airbag coating, which adopts the following technical solution: A method for preparing an anti-aging and tearing airbag coating comprises the following steps: (1) According to the formula amount of component A, vinyl silicone oil and silicone chain extender are taken, stirred and mixed at 200-300 rpm for 10-20 minutes, and then silicone crosslinking agent, inhibitor and silane coupling agent are added, and mixed for another 10-15 minutes to prepare component A; (2) Add vinyl fluorinated silicone oil, catalyst, tackifier, and antioxidant DW in order according to the formula of component B, and stir at 200-300 rpm for 20-30 minutes under normal pressure to prepare component B; (3) Component A and component B are mixed uniformly in a weight ratio of 1:1 to obtain a coating liquid, which is applied to the surface of a substrate and cured to obtain an anti-aging and tear-resistant airbag coating.

[0015] By mixing, coating, and curing components A and B, the selection and matching of the components in the formula and the optimization of the dosage, as well as the setting of parameters in the preparation method, it is ensured that the film after the product is cured has the characteristics of being thinner, having good flatness, good tensile properties and good tearing properties, and it is low in cost, simple in preparation method, and easy to use.

[0016] In a specific embodiment, the curing process is performed at a temperature of 160-180° C. and a curing time of 1-3 min.

[0017] In summary, this application has the following beneficial effects: 1. A cross-linking framework is provided by reacting vinyl-terminated polydimethylsiloxane with phenyl vinyl silicone oil and hydrogen-containing silicone oil. The shielding effect of phenyl on the surrounding groups improves the chemical stability of the resin to a certain extent. After the vinyl and hydrogen-containing groups form cross-linking and curing, the conjugated electrons between the phenyl groups further improve this effect, reduce the chemical activity of the resin, improve the stability and strength of the coating, enhance the anti-aging performance of the material, and have strong solvent resistance, water resistance, ablation resistance, high temperature resistance and other excellent properties; the inventors also added vinyl fluorinated silicone oil to the coating, and found that the addition of phenyl vinyl silicone oil and vinyl fluorinated silicone oil significantly improved the coating resistance compared with the addition of phenyl vinyl silicone oil and vinyl fluorinated silicone oil alone. The effects of anti-aging, water and oil resistance may be due to the addition of vinyl fluorinated silicone oil. The fluorinated groups in the vinyl fluorinated silicone oil are electron-withdrawing groups. The vinyl group promotes the cross-linking density, so that the vinyl fluorinated silicone oil can produce intermolecular interaction forces with the above cross-linking framework, and be embedded or attached to the surface of the cross-linking network system; the fluorinated groups such as trifluoromethyl are dispersed in claws due to the steric hindrance effect between F and F, and the fluorinated groups and phenyl groups are in different silane side chains, so that some F atoms are exposed on the surface of the cross-linking system, and some are dispersed between the benzene rings, and are not shielded by the steric hindrance of the benzene rings, giving full play to the hydrophobic and oleophobic properties of the vinyl fluorinated silicone oil and the anti-aging and stability of the phenyl group, and improving the cross-linking density of the system and the anti-tearing effect. In addition, the wear resistance, heat stability, oil resistance, corrosion resistance, etc. of the coating are also improved, and the service life of the coating is increased.

[0018] 2. Phenyl vinyl silicone oil, under the appropriate addition ratio, can cooperate with organosilicon fluorinated silicone oil to play a better anti-aging effect, which helps to make the coating material wear resistance and UV aging resistance test performance excellent, so that the coating material can maintain better stability in the face of a more complex external environment and is not easily destroyed, thereby extending the service life of the material. The applicant found that when the phenyl content in the system is insufficient, the side chain structure is not tight enough, the adjacent phenyl forces are small, the conjugated shielding effect is small, and the overall stability and anti-aging performance of the cross-linked framework structure are affected; when the phenyl content in the system is too high, the side chain phenyl is too much, which is not conducive to the cross-linking reaction of the cross-linking system, resulting in a decrease in the strength of the cross-linking system, which is not conducive to the formation of a dense coating, thereby reducing the anti-aging performance, and too much phenyl is easy to cause the shielding of the fluorinated group and reduce the hydrophobic and oleophobic performance. In addition, too many benzene rings also affect the flexibility of the coating; by adding a silane coupling agent, the adhesion of the coating is further improved to avoid coating peeling. DETAILED DESCRIPTION

[0019] The present application is further described in detail below in conjunction with embodiments.

[0020] Some of the raw materials used in the preparation examples and embodiments: The vinyl-terminated polydimethylsiloxane is a vinyl double-terminated polydimethylsiloxane with a viscosity of 2000mPa.s, purchased from Hubei Shuaiyan Ligao Biotechnology Co., Ltd.; the phenyl vinyl silicone oil model is lnb-1163; the terminal vinyl fluorinated silicone oil is a terminal vinyl polymethyltrifluoropropylsiloxane with a viscosity of 1000mPa.s, purchased from Wuhan Huaxiang Kejie Biotechnology Co., Ltd.; the diallyl maleate is purchased from Wuhan Kemik Biotechnology Co., Ltd.; the isopropyl tri(dioctyl pyrophosphate) titanate model is HY-201; the hydrogen-terminated polydimethylsiloxane has a viscosity of 40mPa.s, purchased from Hubei Langbowan Biotechnology Co., Ltd.; the polymethyl hydrogensiloxane is purchased from Wuhan Jixin Yibang Biotechnology Co., Ltd., model: 63148-57-2; the catalyst is a Castaplatin catalyst, specifically model: FDW25.

[0021] The raw materials used in the examples and comparative examples that are not otherwise specified are all conventional products that can be purchased from the market. Example

[0022] Example 1 An anti-aging and tear-resistant airbag coating comprises a component A and a component B, wherein the component A comprises the following components in parts by weight: 650 g of vinyl silicone oil, 150 g of an organosilicon chain extender, 30 g of an organosilicon crosslinking agent, 0.5 g of an inhibitor, and 30 g of a silane coupling agent; the component B comprises the following components in parts by weight: 400 g of vinyl fluorinated silicone oil, 4 g of a catalyst, 15 g of a tackifier, and 10 g of an antioxidant DW, wherein the vinyl silicone oil is vinyl-terminated polydimethylsiloxane and phenyl vinyl silicone oil, and the mass ratio of the vinyl-terminated polydimethylsiloxane to the phenyl vinyl silicone oil is 5:1; the vinyl fluorinated silicone oil is vinyl-terminated polymethyltrifluoropropylsiloxane; and the silane coupling agents are KH560 and KH570 in a mass ratio of 1:2.

[0023] (1) Add vinyl silicone oil and silicone chain extender according to the formula amount of component A, mix at 300 rpm for 10 minutes, then add silicone crosslinker, inhibitor, and silane coupling agent, and mix for another 10 minutes to prepare component A.

[0024] (2) adding vinyl fluorinated silicone oil, catalyst, tackifier, and antioxidant DW in order according to the formula of component B, stirring at 300 rpm for 20 minutes under normal pressure to prepare component B; (3) Component A and component B are mixed uniformly in a weight ratio of 1:1 to obtain a coating liquid, which is applied to the surface of a substrate at a curing temperature of 180° C. for a curing time of 1 min to obtain an anti-aging and anti-tearing airbag coating.

[0025] Example 2 An anti-aging and tear-resistant airbag coating comprises a component A and a component B, wherein the component A comprises the following components in parts by weight: 700 g of vinyl silicone oil, 120 g of an organosilicon chain extender, 55 g of an organosilicon crosslinker, 1 g of an inhibitor, and 25 g of a silane coupling agent; Component B includes the following components in parts by weight: 600g of vinyl fluorinated silicone oil, 7g of catalyst, 30g of tackifier, and 20g of antioxidant DW; wherein the vinyl silicone oil is vinyl-terminated polydimethylsiloxane and phenyl vinyl silicone oil, and the mass ratio of vinyl-terminated polydimethylsiloxane to phenyl vinyl silicone oil is 5:1; the vinyl fluorinated silicone oil is vinyl-terminated polymethyltrifluoropropylsiloxane; and the silane coupling agent is KH560 and KH570 in a mass ratio of 1:2.

[0026] (1) Add vinyl silicone oil and silicone chain extender according to the formula amount of component A, mix at 300 rpm for 10 minutes, then add silicone crosslinker, inhibitor, and silane coupling agent, and mix for another 10 minutes to prepare component A.

[0027] (2) adding vinyl fluorinated silicone oil, catalyst, tackifier, and antioxidant DW in order according to the formula of component B, stirring at 300 rpm for 20 minutes under normal pressure to prepare component B; (3) Component A and component B are mixed uniformly in a weight ratio of 1:1 to obtain a coating liquid, which is applied to the surface of a substrate at a curing temperature of 180° C. for a curing time of 1 min to obtain an anti-aging and anti-tearing airbag coating.

[0028] Example 3 An anti-aging and tear-resistant airbag coating comprises a component A and a component B, wherein the component A comprises the following components in parts by weight: 850 g of vinyl silicone oil, 140 g of an organosilicon chain extender, 55 g of an organosilicon crosslinker, 1 g of an inhibitor, and 25 g of a silane coupling agent; Component B includes the following components in parts by weight: 800g of vinyl fluorinated silicone oil, 1g of catalyst, 30g of tackifier, and 30g of antioxidant DW; wherein the vinyl silicone oil is vinyl-terminated polydimethylsiloxane and phenyl vinyl silicone oil, and the mass ratio of vinyl-terminated polydimethylsiloxane to phenyl vinyl silicone oil is 5:1; the vinyl fluorinated silicone oil is vinyl-terminated polymethyltrifluoropropylsiloxane; and the silane coupling agent is KH560 and KH570 in a mass ratio of 1:2.

[0029] (1) Add vinyl silicone oil and silicone chain extender according to the formula amount of component A, mix at 300 rpm for 10 minutes, then add silicone crosslinker, inhibitor, and silane coupling agent, and mix for another 10 minutes to prepare component A.

[0030] (2) adding vinyl fluorinated silicone oil, catalyst, tackifier, and antioxidant DW in order according to the formula of component B, stirring at 300 rpm for 20 minutes under normal pressure to prepare component B; (3) Component A and component B are mixed uniformly in a weight ratio of 1:1 to obtain a coating liquid, which is applied to the surface of a substrate at a curing temperature of 180° C. for a curing time of 1 min to obtain an anti-aging and anti-tearing airbag coating.

[0031] Example 4 An anti-aging and tear-resistant airbag coating comprises a component A and a component B, wherein the component A comprises the following components in parts by weight: 700 g of vinyl silicone oil, 120 g of an organosilicon chain extender, 55 g of an organosilicon crosslinker, 1 g of an inhibitor, and 25 g of a silane coupling agent; Component B includes the following components in parts by weight: 600g of vinyl fluorinated silicone oil, 7g of catalyst, 30g of tackifier, and 20g of antioxidant DW; wherein the vinyl silicone oil is vinyl-terminated polydimethylsiloxane and phenyl vinyl silicone oil, and the mass ratio of vinyl-terminated polydimethylsiloxane to phenyl vinyl silicone oil is 8:1; the vinyl fluorinated silicone oil is vinyl-terminated polymethyltrifluoropropylsiloxane; and the silane coupling agent is KH560 and KH570 in a mass ratio of 1:2.

[0032] (1) Add vinyl silicone oil and silicone chain extender according to the formula amount of component A, mix at 300 rpm for 10 minutes, then add silicone crosslinker, inhibitor, and silane coupling agent, and mix for another 10 minutes to prepare component A.

[0033] (2) adding vinyl fluorinated silicone oil, catalyst, tackifier, and antioxidant DW in order according to the formula of component B, stirring at 300 rpm for 20 minutes under normal pressure to prepare component B; (3) Component A and component B are mixed uniformly in a weight ratio of 1:1 to obtain a coating liquid, which is applied to the surface of a substrate at a curing temperature of 180° C. for a curing time of 1 min to obtain an anti-aging and anti-tearing airbag coating.

[0034] Example 5 An anti-aging and tear-resistant airbag coating comprises a component A and a component B, wherein the component A comprises the following components in parts by weight: 700 g of vinyl silicone oil, 120 g of an organosilicon chain extender, 55 g of an organosilicon crosslinker, 1 g of an inhibitor, and 25 g of a silane coupling agent; Component B includes the following components in parts by weight: 600g of vinyl fluorinated silicone oil, 7g of catalyst, 30g of tackifier, and 20g of antioxidant DW; wherein the vinyl silicone oil is vinyl-terminated polydimethylsiloxane and phenyl vinyl silicone oil, and the mass ratio of vinyl-terminated polydimethylsiloxane to phenyl vinyl silicone oil is 6:3; the vinyl fluorinated silicone oil is vinyl-terminated polymethyltrifluoropropylsiloxane; and the silane coupling agent is KH560 and KH570 in a mass ratio of 1:2.

[0035] (1) Add vinyl silicone oil and silicone chain extender according to the formula amount of component A, mix at 300 rpm for 10 minutes, then add silicone crosslinker, inhibitor, and silane coupling agent, and mix for another 10 minutes to prepare component A.

[0036] (2) adding vinyl fluorinated silicone oil, catalyst, tackifier, and antioxidant DW in order according to the formula of component B, stirring at 300 rpm for 20 minutes under normal pressure to prepare component B; (3) Component A and component B are mixed uniformly in a weight ratio of 1:1 to obtain a coating liquid, which is applied to the surface of a substrate at a curing temperature of 180° C. for a curing time of 1 min to obtain an anti-aging and anti-tearing airbag coating.

[0037] Example 6 An anti-aging and tear-resistant airbag coating comprises a component A and a component B, wherein the component A comprises the following components in parts by weight: 700 g of vinyl silicone oil, 120 g of an organosilicon chain extender, 55 g of an organosilicon crosslinker, 1 g of an inhibitor, and 25 g of a silane coupling agent; Component B includes the following components in parts by weight: 600g of vinyl fluorinated silicone oil, 7g of catalyst, 30g of tackifier, and 20g of antioxidant DW; wherein the vinyl silicone oil is vinyl-terminated polydimethylsiloxane and phenyl vinyl silicone oil, and the mass ratio of vinyl-terminated polydimethylsiloxane to phenyl vinyl silicone oil is 10:1; the vinyl fluorinated silicone oil is vinyl-terminated polymethyltrifluoropropylsiloxane; and the silane coupling agent is KH560 and KH570 in a mass ratio of 1:2.

[0038] (1) Add vinyl silicone oil and silicone chain extender according to the formula amount of component A, mix at 300 rpm for 10 minutes, then add silicone crosslinker, inhibitor, and silane coupling agent, and mix for another 10 minutes to prepare component A.

[0039] (2) adding vinyl fluorinated silicone oil, catalyst, tackifier, and antioxidant DW in order according to the formula of component B, stirring at 300 rpm for 20 minutes under normal pressure to prepare component B; (3) Component A and component B are mixed uniformly in a weight ratio of 1:1 to obtain a coating liquid, which is applied to the surface of a substrate at a curing temperature of 180° C. for a curing time of 1 min to obtain an anti-aging and anti-tearing airbag coating.

[0040] Comparative Example 1 An anti-aging and tear-resistant airbag coating comprises a component A and a component B, wherein the component A comprises the following components in parts by weight: 700 g of vinyl silicone oil, 120 g of an organosilicon chain extender, 55 g of an organosilicon crosslinker, 1 g of an inhibitor, and 25 g of a silane coupling agent; wherein the vinyl silicone oil is vinyl-terminated polydimethylsiloxane; and the silane coupling agent is KH560 and KH570 in a mass ratio of 1:2; Component B includes the following components in parts by weight: 600 g of vinyl fluorinated silicone oil, 7 g of catalyst, 30 g of tackifier, and 20 g of antioxidant DW; wherein the vinyl fluorinated silicone oil is vinyl-terminated polymethyltrifluoropropylsiloxane.

[0041] (1) Add vinyl silicone oil and silicone chain extender according to the formula amount of component A, mix at 300 rpm for 10 minutes, then add silicone crosslinker, inhibitor, and silane coupling agent, and mix for another 10 minutes to prepare component A.

[0042] (2) adding vinyl fluorinated silicone oil, catalyst, tackifier, and antioxidant DW in order according to the formula of component B, stirring at 300 rpm for 20 minutes under normal pressure to prepare component B; (3) Component A and component B are mixed uniformly in a weight ratio of 1:1 to obtain a coating liquid, which is applied to the surface of a substrate at a curing temperature of 180° C. for a curing time of 1 min to obtain an anti-aging and anti-tearing airbag coating.

[0043] Comparative Example 2 An anti-aging and tear-resistant airbag coating comprises a component A and a component B, wherein the component A comprises the following components in parts by weight: 700 g of vinyl silicone oil, 120 g of an organosilicon chain extender, 55 g of an organosilicon cross-linking agent, 1 g of an inhibitor, and 25 g of a silane coupling agent; wherein the vinyl silicone oil is phenyl vinyl silicone oil; and the silane coupling agent is KH560 and KH570 in a mass ratio of 1:2.

[0044] Component B includes the following components in parts by weight: 600 g of vinyl fluorinated silicone oil, 7 g of catalyst, 30 g of tackifier, and 20 g of antioxidant DW; the vinyl fluorinated silicone oil is vinyl-terminated polymethyltrifluoropropylsiloxane.

[0045] (1) Add vinyl silicone oil and silicone chain extender according to the formula amount of component A, mix at 300 rpm for 10 minutes, then add silicone crosslinker, inhibitor, and silane coupling agent, and mix for another 10 minutes to prepare component A.

[0046] (2) adding vinyl fluorinated silicone oil, catalyst, tackifier, and antioxidant DW in order according to the formula of component B, stirring at 300 rpm for 20 minutes under normal pressure to prepare component B; (3) Component A and component B are mixed uniformly in a weight ratio of 1:1 to obtain a coating liquid, which is applied to the surface of a substrate at a curing temperature of 180° C. for a curing time of 1 min to obtain an anti-aging and anti-tearing airbag coating.

[0047] Comparative Example 3 An anti-aging and tear-resistant airbag coating comprises a component A and a component B, wherein the component A comprises the following components in parts by weight: 700 g of vinyl silicone oil, 120 g of an organosilicon chain extender, 55 g of an organosilicon crosslinker, 1 g of an inhibitor, and 25 g of a silane coupling agent; Component B includes the following components in parts by weight: 600 g of vinyl-terminated polydimethylsiloxane, 7 g of catalyst, 30 g of tackifier, and 20 g of antioxidant DW; wherein the vinyl silicone oil is vinyl-terminated polydimethylsiloxane and phenyl vinyl silicone oil, and the mass ratio of vinyl-terminated polydimethylsiloxane to phenyl vinyl silicone oil is 5:1; and the silane coupling agent is KH560 and KH570 in a mass ratio of 1:2.

[0048] (1) Add vinyl silicone oil and silicone chain extender according to the formula amount of component A, mix at 300 rpm for 10 minutes, then add silicone crosslinker, inhibitor, and silane coupling agent, and mix for another 10 minutes to prepare component A.

[0049] (2) adding vinyl fluorinated silicone oil, catalyst, tackifier, and antioxidant DW in order according to the formula of component B, stirring at 300 rpm for 20 minutes under normal pressure to prepare component B; (3) Component A and component B are mixed uniformly in a weight ratio of 1:1 to obtain a coating liquid, which is applied to the surface of a substrate at a curing temperature of 180° C. for a curing time of 1 min to obtain an anti-aging and anti-tearing airbag coating.

[0050] Comparative Example 4 An anti-aging and tear-resistant airbag coating comprises a component A and a component B, wherein the component A comprises the following components in parts by weight: 820 g of vinyl silicone oil, 55 g of an organic silicon crosslinking agent, 1 g of an inhibitor, and 25 g of a silane coupling agent; Component B includes the following components in parts by weight: 600g of vinyl fluorinated silicone oil, 7g of catalyst, 30g of tackifier, and 20g of antioxidant DW; wherein the vinyl silicone oil is vinyl-terminated polydimethylsiloxane and phenyl vinyl silicone oil, and the mass ratio of vinyl-terminated polydimethylsiloxane to phenyl vinyl silicone oil is 5:1; the vinyl fluorinated silicone oil is vinyl-terminated polymethyltrifluoropropylsiloxane; and the silane coupling agent is KH560 and KH570 in a mass ratio of 1:2.

[0051] (1) Add vinyl silicone oil and silicone chain extender according to the formula amount of component A, mix at 300 rpm for 10 minutes, then add silicone crosslinker, inhibitor, and silane coupling agent, and mix for another 10 minutes to prepare component A.

[0052] (2) adding vinyl fluorinated silicone oil, catalyst, tackifier, and antioxidant DW in order according to the formula of component B, stirring at 300 rpm for 20 minutes under normal pressure to prepare component B; (3) Component A and component B are mixed uniformly in a weight ratio of 1:1 to obtain a coating liquid, which is applied to the surface of a substrate at a curing temperature of 180° C. for a curing time of 1 min to obtain an anti-aging and anti-tearing airbag coating.

[0053] Performance Testing An anti-aging and tear-resistant airbag coating liquid prepared in the embodiment and the comparative example was coated on the surface of a nylon 66 substrate to form a thin film, and the performance of the film was tested using the following method: a. Tensile strength: Tested in accordance with GB / T528-1998; b. Tear strength: Tested in accordance with GB / T528-1999; c. Anti-aging test: After the airbag coating was subjected to a heat and humidity aging treatment for 3000 hours in a high and low temperature heat and humidity chamber at a temperature of 50°C and a humidity of 95%, the experimental results show that the airbag coating has excellent aging resistance. The comparison results are shown in Table 1 below: Table 1 Performance test results It can be seen from Table 1 that the anti-aging and tear-resistant airbag coatings obtained in the above embodiments meet the safety requirements of the driver or passenger in case of airbag explosion; compared with Comparative Examples 1-2, Examples 2 and Examples 4-6, it can be seen that the tear strength and tensile strength of the anti-aging and tear-resistant airbag coating obtained in Example 2 before and after wet-heat aging are better than those of Comparative Examples 1-2 and Examples 4-6; analysis shows that the reaction of vinyl-terminated polydimethylsiloxane, phenyl vinyl silicone oil and hydrogen-containing silicone oil provides a conjugated cross-linked framework, enhances the electronic shielding effect between the system's organic silicone oils, reduces the interaction between different molecules, and enhances the anti-aging performance of the material; the applicant found that when the phenyl content in the system is too large or too small, it will affect the overall mechanical properties of the coating material, resulting in affecting the overall stability and tear resistance of the cross-linked framework structure and the aging resistance of the material is not ideal.

[0054] Comparison of Example 2 and Comparative Example 3 shows that the tear strength and tensile strength of an anti-aging and tear-resistant airbag coating obtained in Example 2 before and after wet heat aging are better than those of Comparative Example 3. It is analyzed that the addition of vinyl fluorinated silicone oil, the fluorinated group in the vinyl fluorinated silicone oil is an electron-withdrawing group, and the vinyl promotes the cross-linking density, so that the vinyl fluorinated silicone oil can produce intermolecular interaction forces with the above-mentioned cross-linking framework, embedded or attached to the surface of the cross-linked network system; trifluoromethyl and other fluorinated groups are claw-shaped and dispersed due to the steric effect between F and F, and the fluorinated group and the phenyl group are in different silane side chains, so that some F atoms are exposed to the surface of the cross-linking system, and are partially dispersed between the benzene rings, and are not shielded by the steric effect of the benzene ring, giving full play to the hydrophobic and oleophobic properties of the vinyl fluorinated silicone oil and the anti-aging and stability of the phenyl group, and improving the cross-linking density of the system, and improving the tear resistance effect. In addition, the wear resistance, heat stability, oil resistance, corrosion resistance, etc. of the coating are also improved, and the service life of the coating is improved.

[0055] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.

Claims

1. An anti-aging and tear-resistant airbag coating, characterized in that: The invention comprises component A and component B, wherein component A comprises the following components in parts by weight: 65-85 parts of vinyl silicone oil, 12-15 parts of organosilicon chain extender, 3-5.5 parts of organosilicon crosslinker, 0.05-0.1 parts of inhibitor and 2.5-3 parts of silane coupling agent; component B comprises the following components in parts by weight: 40-80 parts of vinyl fluorine-containing silicone oil, 0.1-0.7 parts of catalyst, 1.5-3 parts of tackifier and 1-3 parts of antioxidant DW; the vinyl silicone oil of component A comprises vinyl-terminated polydimethylsiloxane and phenyl vinyl silicone oil.

2. The anti-aging and tear-resistant airbag coating according to claim 1, characterized in that: The mass ratio of the vinyl-terminated polydimethylsiloxane to the phenyl vinyl silicone oil is (5-8):

1.

3. The anti-aging and tear-resistant airbag coating according to claim 1, characterized in that: The vinyl fluorine-containing silicone oil of the B component is a vinyl-terminated fluorine-containing silicone oil.

4. The anti-aging and tear-resistant airbag coating according to claim 1, characterized in that: The inhibitor is diallyl maleate; and the organosilicon crosslinking agent is polymethyl hydrogen siloxane.

5. The anti-aging and tear-resistant airbag coating according to claim 1, characterized in that: The tackifier is isopropyl tri(dioctyl pyrophosphate) titanate.

6. The anti-aging and tear-resistant airbag coating according to claim 1, characterized in that: The organosilicon chain extender is hydrogen-terminated polydimethylsiloxane.

7. A method for preparing an anti-aging and tear-resistant airbag coating according to claims 1-6, characterized in that: The steps include: (1) According to the formula amount of component A, vinyl silicone oil and silicone chain extender are taken, stirred and mixed at 200-300 rpm for 10-20 minutes, and then silicone crosslinking agent, inhibitor and silane coupling agent are added, and mixed for another 10-15 minutes to prepare component A; (2) Add vinyl fluorinated silicone oil, catalyst, tackifier, and antioxidant DW in order according to the formula of component B, and stir at 200-300 rpm for 20-30 minutes under normal pressure to prepare component B; (3) Component A and component B are mixed uniformly in a weight ratio of 1:1 to obtain a coating liquid, which is applied to the surface of a substrate and cured to obtain an anti-aging and tear-resistant airbag coating.

8. The method for preparing an anti-aging and tear-resistant airbag coating according to claim 7, characterized in that: The curing treatment is performed at a temperature of 160-180° C. and a curing time of 1-3 minutes.

Citation Information

Patent Citations

  • Novel coating silica gel material for automobile safety airbag and preparation method thereof

    CN103756561A

  • Organic silicon scratch-resistant antifouling coating for synthetic leather and preparation method of organic silicon scratch-resistant antifouling coating

    CN114716910A

  • Two-component silicone rubber anti-pollution flashover coating for insulation protection of power system as well as preparation method and application of two-component silicone rubber anti-pollution flashover coating

    CN115851125A

  • Silicone composition and process that is useful for improving the tear strength and the combing strength of an inflatable bag for protecting an occupant of a vehicle

    CN1890426A

  • Silicone coatings for air bags

    US20220356370A1

Cited By

  • Wear-resistant and corrosion-resistant coating and preparation method thereof