Preservative for metal material surface
Through imidazoline derivatives and benzotriazole compounding and microcapsule technology, a preservative for metal material surface was prepared, which solved the problem of cracks and peeling of existing preservatives, and achieved long-term protection and self-containment Repair significantly improves anti-corrosion effect and durability.
Patent Information
- Application Number
- CN202411418649.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-12
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing metal preservatives are prone to cracks and peeling during use, resulting in poor anti-corrosion effect and inability to continuously and effectively protect metal materials.
Imidazoline derivatives and benzotriazole are combined into anticorrosion components, combined with modified corrosion inhibitors, fillers and film-forming agents, and prepared modified corrosion inhibitors and film-forming agents through microcapsule technology to form multiple protective films , realize self-healing and dense protection.
It significantly improves the adhesion and durability of the preservative, enhances the protection effect on metal surfaces, can maintain good performance in various environments, extends the effectiveness of the preservative and reduces costs.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of metal corrosion inhibitors, and more specifically, to a corrosion inhibitor for the surface of metal materials. Background Art
[0002] Metal corrosion is the phenomenon that metal materials are damaged by the surrounding medium, which is particularly evident in the form of metal rust. This process involves complex chemical or electrochemical multiphase reactions on the metal surface, which causes the metal to transform into an oxidized state, thereby significantly reducing the key mechanical properties of the metal material, such as strength, plasticity and toughness. In addition, corrosion will also change the original geometry of metal parts, increase wear between parts, and adversely affect physical properties such as electrical and optical properties, ultimately shortening the service life of related equipment and even causing serious safety accidents such as fire and explosion.
[0003] In recent years, in order to deal with the problem of metal corrosion, people have continuously explored and applied a variety of protection technologies. One of the most effective and economical methods is to form an anti-corrosion isolation film on the metal surface to build a barrier that can effectively isolate the direct contact between the corrosive medium and the metal substrate. However, in practical applications, the existing anti-corrosion isolation film will generate many small cracks during use due to changes in the environment (such as temperature and humidity, acidity and alkalinity changes) or mechanical properties (such as stress concentration, vibration) and other factors. These small cracks gradually spread and expand in the atmosphere, thereby accelerating the corrosion of the metal. Therefore, a metal preservative is needed that can play a role of continuous release and long-term protection to solve the problems of the existing technology that is prone to cracking, peeling, and poor anti-corrosion effect. Summary of the invention
[0004] In order to solve the technical problems mentioned in the background technology, the present application provides a corrosion inhibitor for the surface of metal materials.
[0005] In the first aspect, the present application provides a corrosion inhibitor for the surface of a metal material, which adopts the following technical solution: A corrosion inhibitor for the surface of a metal material comprises the following raw materials in parts by weight: 2-5 parts of an anticorrosive component, 1-2 parts of a modified corrosion inhibitor, 2-3 parts of a filler, 1-1.5 parts of a film former, 1-2 parts of an auxiliary agent, and 50-60 parts of water.
[0006] Preferably, the raw materials include the following parts by weight: 3.5 parts of the antiseptic component, 1.5 parts of the modified corrosion inhibitor, 2.5 parts of the filler, 1.25 parts of the film former, 1.5 parts of the auxiliary agent, and 55 parts of water.
[0007] Preferably, the antiseptic component is prepared by compounding an imidazoline derivative, sodium nitrite and benzotriazole in a mass ratio of 18-20:20-25:5-8.
[0008] Preferably, the preparation of the modified corrosion inhibitor comprises the following steps: Step A, preparing a core material solution: dispersing zinc phosphate, sodium molybdate and montmorillonite in water; Step B, preparing a wall material solution: dispersing polyvinyl alcohol, polyvinyl pyrrolidone and an emulsifier in 80-90° C. water; Step C, polymerization reaction: adding the core material solution to the wall material solution, stirring while adding, for 3-5 hours, to obtain a mixed solution A; Step D, cross-linking: add a cross-linking agent to the mixed solution A, dry at 60-80° C. until the humidity is less than 10%, to obtain a modified corrosion inhibitor.
[0009] Preferably, in step A, the mass ratio of zinc phosphate, sodium molybdate and montmorillonite is 30-40:15-20:18-22.
[0010] Preferably, the mass percentage concentration of the core material solution in step A is 20-25%.
[0011] Preferably, in step B, the mass ratio of polyvinyl alcohol, polyvinyl pyrrolidone and emulsifier A is 2-3:1-2:0.2-0.5.
[0012] Preferably, the mass percentage concentration of the wall material solution in step B is 10-18%.
[0013] Preferably, in step C, the mass ratio of the core material solution to the wall material solution is 1-1.5:2-3.
[0014] Preferably, the filler consists of diatomaceous earth, kaolin and calcium carbonate in a mass ratio of 1-2:2-4:1-3.
[0015] Preferably, the mass percentage concentration of the gelatin solution is 8-10%, the mass percentage concentration of the alum solution is 2-3%, and the mass percentage concentration of the glutaraldehyde solution is 5.5-6%.
[0016] Preferably, the gelatin solution is prepared by adding 80-100 g of gelatin to 1 L of water, controlling the water temperature to 60-70° C., and stirring thoroughly.
[0017] Preferably, the alum solution is prepared by adding 20-30 g of alum into 1 L of water and stirring thoroughly at room temperature.
[0018] Preferably, the glutaraldehyde solution is prepared by adding 55-60 g of glutaraldehyde into 1 L of water and stirring thoroughly at room temperature.
[0019] In a second aspect, the present application also provides a method for preparing a corrosion inhibitor for the surface of a metal material, comprising the following preparation steps: Step a: After mixing the anticorrosive component and the modified corrosion inhibitor according to weight parts, add them into 50-60°C water, control the stirring speed to 60-80rpm, stir for 30-40min, and stir thoroughly to obtain a mixed solution B; Step b: Add filler, film-forming agent and auxiliary agent to mixed solution B, control the stirring speed to 80-100 rpm, stir for 40-60 min, filter, cool and package in a sealed container to obtain the preservative for the surface of metal materials.
[0020] In summary, this application has the following beneficial effects: This application uses imidazoline derivatives and benzotriazole to easily adsorb on the metal surface to form a protective film, and sodium nitrite as an anodic corrosion inhibitor, which can inhibit the anodic dissolution process. The three compound uses can complement each other to form multiple protective effects. The modified corrosion inhibitor is prepared by microcapsule technology, which is more accurate in the use of preservatives, reduces unnecessary waste, extends the shelf life of preservatives, and also reduces costs; the presence of microcapsules can enhance the overall uniformity and stability, and the interaction between the corrosion inhibitor in the microcapsules and the membrane material can enhance the cross-linking density of the membrane, improve its density and uniformity, thereby improving the overall protective performance. The corrosion inhibitor after microencapsulation can be automatically released when the anticorrosive film is damaged, fill the damaged area, and achieve self-repair. Even when there is minor damage on the surface of the anticorrosive film, the corrosion inhibitor in the microcapsule can continue to play a role to prevent further spread of corrosion. This self-repair function can greatly improve the durability of the metal.
[0021] The filler in the present application utilizes the pore structure of diatomaceous earth and kaolin to effectively absorb harmful substances in the corrosive medium, and the buffering effect of calcium carbonate neutralizes the acidic medium, adjusts the pH value, and protects the metal surface from corrosion. The film-forming agent is prepared by compounding gelatin solution, alum solution and glutaraldehyde solution. Gelatin has good film-forming properties, alum can promote the cross-linking of gelatin, and glutaraldehyde can also react with functional groups such as amino groups in gelatin to form a more stable three-dimensional network structure, which can form a dense protective layer on the metal surface, improve the strength and stability of the film, and improve the flexibility of the film, so that it can maintain good performance in various environments. DETAILED DESCRIPTION
[0022] The present application is further described in detail below with reference to the embodiments.
[0023] Embodiment 1-3 provides a corrosion inhibitor for the surface of a metal material.
[0024] The polyvinyl alcohol used in the examples of the present invention and the comparative examples was purchased from Guangzhou Qihua Chemical Co., Ltd. (product model BP24, average degree of polymerization: 2400-2500); polyvinyl pyrrolidone was purchased from Jiaozuo Zhongwei Special Products Pharmaceutical Co., Ltd. (product model industrial grade PVP K60); fatty acid polyoxyethylene ether was purchased from Jiangsu Santuo New Materials Co., Ltd. (product model A-105, HLB value 8.5-9.5); Tween-80 and Span-80 were both purchased from Xingtai Xinlanxing Technology Co., Ltd.
[0025] Example 1
[0026] A corrosion inhibitor for the surface of a metal material comprises the following raw materials in parts by weight: 2 parts of an anticorrosive component, 1 part of a modified corrosion inhibitor, 2 parts of a filler, 1 part of a film former, 1 part of an auxiliary agent, and 50 parts of water.
[0027] Wherein, the preparation of the modified corrosion inhibitor comprises the following steps: Step A, preparing a core material solution: dispersing zinc phosphate, sodium molybdate and montmorillonite in a mass ratio of 30:15:18 in water, stirring with a high-speed stirrer, setting the speed to 1000 rpm, stirring at room temperature for 20 minutes, and controlling the mass percentage concentration of the core material solution to be 20%; Step B, preparing a wall material solution: dispersing polyvinyl alcohol, polyvinyl pyrrolidone and polyoxyethylene ether in a mass ratio of 2:1:0.2 in 80°C water, stirring with a high-speed stirrer at a speed of 2000 rpm for 30 minutes, and controlling the mass percentage concentration of the wall material solution to be 10%; Step C, polymerization reaction: adding the core material solution to the wall material solution, controlling the mass ratio of the core material solution to the wall material solution to be 1:2, stirring while adding, controlling the stirring speed to be 300 rpm, stirring for 3 hours, to obtain a mixed solution A; Step D, cross-linking: glutaraldehyde was added to the mixed solution A, stirred at 200 rpm for 5 min, the amount of glutaraldehyde was controlled to be 1% of the total mass of the mixed solution A, and dried at 60° C. until the humidity was 8%, to obtain a modified corrosion inhibitor.
[0028] A method for preparing an anticorrosive agent for the surface of a metal material comprises the following steps: Step a: After mixing the anti-corrosion component and the modified corrosion inhibitor in parts by weight, adding them into 50° C. water, controlling the stirring speed at 60 rpm, stirring for 30 minutes, and fully stirring to obtain a mixed solution B, wherein the anti-corrosion component is prepared by compounding 2-dodecyl imidazoline, sodium nitrite and benzotriazole in a mass ratio of 18:20:5; Step b: adding a filler, a film-forming agent and sodium benzoate to the mixed solution B, controlling the stirring speed to 80 rpm, stirring for 40 minutes, filtering, cooling and packaging in a closed container to obtain a preservative for the surface of a metal material, wherein the filler is composed of diatomaceous earth, kaolin and calcium carbonate in a mass ratio of 1:2:1, the film-forming agent is compounded by a gelatin solution, an alum solution and a glutaraldehyde solution in a mass ratio of 1:2:0.2, the gelatin solution is prepared by adding 80g of gelatin to 1L of water, controlling the water temperature to 60°C, and fully stirring, the alum solution is prepared by adding 20g of alum to 1L of water, and fully stirring at room temperature, and the glutaraldehyde solution is prepared by adding 55g of glutaraldehyde to 1L of water, and fully stirring at room temperature.
[0029] Example 2
[0030] A corrosion inhibitor for the surface of a metal material comprises the following raw materials in parts by weight: 4 parts of an anticorrosive component, 1.5 parts of a modified corrosion inhibitor, 2.5 parts of a filler, 1.25 parts of a film former, 1.5 parts of an auxiliary agent, and 55 parts of water.
[0031] Wherein, the preparation of the modified corrosion inhibitor comprises the following steps: Step A, preparing a core material solution: dispersing zinc phosphate, sodium molybdate and montmorillonite in a mass ratio of 35:17:20 in water, stirring with a high-speed stirrer, setting the speed to 1250 rpm, stirring at room temperature for 25 minutes, and controlling the mass percentage concentration of the core material solution to be 22%; Step B, preparing a wall material solution: dispersing polyvinyl alcohol, polyvinyl pyrrolidone and Tween-80 in a mass ratio of 2.5:1.5:0.3 in 85°C water, stirring with a high-speed stirrer at a speed of 2250 rpm for 35 minutes, and controlling the mass percentage concentration of the wall material solution to be 14%; Step C, polymerization reaction: adding the core material solution to the wall material solution, controlling the mass ratio of the core material solution to the wall material solution to be 1.25:2.5, stirring while adding, controlling the stirring speed to be 350 rpm, stirring for 4 hours, to obtain a mixed solution A; Step D, cross-linking: glutaraldehyde was added to the mixed solution A, stirred at 250 rpm for 8 min, the amount of glutaraldehyde was controlled to be 2% of the total mass of the mixed solution A, and dried at 70° C. to a humidity of 6% to obtain a modified corrosion inhibitor.
[0032] A method for preparing an anticorrosive agent for the surface of a metal material comprises the following steps: Step a: After mixing the anti-corrosion component and the modified corrosion inhibitor in parts by weight, adding them into 55° C. water, controlling the stirring speed at 70 rpm, stirring for 35 minutes, and fully stirring to obtain a mixed solution B, wherein the anti-corrosion component is prepared by compounding 2-dodecyl imidazoline, sodium nitrite and benzotriazole in a mass ratio of 19:22:6.5; Step b: adding a filler, a film-forming agent and silicone oil to the mixed solution B, controlling the stirring speed to 90 rpm, stirring for 50 minutes, filtering, cooling and packaging in a closed container to obtain a preservative for the surface of a metal material, wherein the filler is composed of diatomaceous earth, kaolin and calcium carbonate in a mass ratio of 1.5:3:2, the film-forming agent is compounded by a gelatin solution, an alum solution and a glutaraldehyde solution in a mass ratio of 1.5:2.5:0.25, the gelatin solution is prepared by adding 90 g of gelatin to 1 L of water, controlling the water temperature to 65°C, and fully stirring, the alum solution is prepared by adding 25 g of alum to 1 L of water, and fully stirring at room temperature, and the glutaraldehyde solution is prepared by adding 58 g of glutaraldehyde to 1 L of water, and fully stirring at room temperature.
[0033] Example 3
[0034] A corrosion inhibitor for the surface of a metal material comprises the following raw materials in parts by weight: 5 parts of an anticorrosive component, 2 parts of a modified corrosion inhibitor, 3 parts of a filler, 1.5 parts of a film former, 2 parts of an auxiliary agent, and 60 parts of water.
[0035] Wherein, the preparation of the modified corrosion inhibitor comprises the following steps: Step A, preparing a core material solution: dispersing zinc phosphate, sodium molybdate and montmorillonite in a mass ratio of 40:20:22 in water, stirring with a high-speed stirrer, setting the speed to 1500 rpm, stirring at room temperature for 30 minutes, and controlling the mass percentage concentration of the core material solution to be 25%; Step B, preparing a wall material solution: dispersing polyvinyl alcohol, polyvinyl pyrrolidone and Span-80 in a mass ratio of 3:2:0.5 in 90°C water, stirring with a high-speed stirrer at a speed of 2500 rpm for 40 minutes, and controlling the mass percentage concentration of the wall material solution to be 18%; Step C, polymerization reaction: adding the core material solution to the wall material solution, controlling the mass ratio of the core material solution to the wall material solution to be 1.5:3, stirring while adding, controlling the stirring speed to be 400 rpm, stirring for 5 hours, and obtaining a mixed solution A; Step D, cross-linking: glutaraldehyde was added to the mixed solution A, stirred at 300 rpm for 10 min, the amount of glutaraldehyde was controlled to be 3% of the total mass of the mixed solution A, and dried at 80° C. until the humidity was 4%, to obtain a modified corrosion inhibitor.
[0036] A method for preparing an anticorrosive agent for the surface of a metal material comprises the following steps: Step a: After mixing the anti-corrosion component and the modified corrosion inhibitor in parts by weight, adding them into 60° C. water, controlling the stirring speed at 80 rpm, stirring for 40 minutes, and fully stirring to obtain a mixed solution B, wherein the anti-corrosion component is prepared by compounding 2-dodecyl imidazoline, sodium nitrite and benzotriazole in a mass ratio of 20:25:8; Step b: adding a filler, a film-forming agent and a polycarboxylate to a mixed solution B, controlling the stirring speed at 100 rpm, stirring for 60 minutes, filtering, cooling and packaging in a sealed container to obtain a preservative for the surface of a metal material, wherein the filler is composed of diatomaceous earth, kaolin and calcium carbonate in a mass ratio of 2:4:3, the film-forming agent is compounded from a gelatin solution, an alum solution and a glutaraldehyde solution in a mass ratio of 2:3:0.3, the gelatin solution is prepared by adding 100 g of gelatin to 1 L of water, controlling the water temperature to 70°C and fully stirring, the alum solution is prepared by adding 30 g of alum to 1 L of water and fully stirring at room temperature, and the glutaraldehyde solution is prepared by adding 60 g of glutaraldehyde to 1 L of water and fully stirring at room temperature.
[0037] Comparative Example 1 A corrosion inhibitor for the surface of a metal material comprises the following raw materials in parts by weight: 2 parts of an anticorrosive component, 1 part of a modified corrosion inhibitor, 2 parts of a filler, 1 part of a film former, 1 part of an auxiliary agent, and 50 parts of water.
[0038] Wherein, the preparation of the modified corrosion inhibitor comprises the following steps: Step A, preparing a core material solution: dispersing zinc phosphate, sodium molybdate and montmorillonite in a mass ratio of 30:15:18 in water, stirring with a high-speed stirrer, setting the speed to 1000 rpm, stirring at room temperature for 20 minutes, and controlling the mass percentage concentration of the core material solution to be 20%; Step B, preparing a wall material solution: dispersing polyvinyl alcohol, polyvinyl pyrrolidone and polyoxyethylene ether in a mass ratio of 2:1:0.2 in 80°C water, stirring with a high-speed stirrer at a speed of 2000 rpm for 30 minutes, and controlling the mass percentage concentration of the wall material solution to be 10%; Step C, polymerization reaction: adding the core material solution to the wall material solution, controlling the mass ratio of the core material solution to the wall material solution to be 1:2, stirring while adding, controlling the stirring speed to be 300 rpm, stirring for 3 hours, to obtain a mixed solution A; Step D, cross-linking: glutaraldehyde was added to the mixed solution A, stirred at 200 rpm for 5 min, the amount of glutaraldehyde was controlled to be 1% of the total mass of the mixed solution A, and dried at 60° C. until the humidity was 8%, to obtain a modified corrosion inhibitor.
[0039] A method for preparing an anticorrosive agent for the surface of a metal material comprises the following steps: Step a: After mixing the anti-corrosion component and the modified corrosion inhibitor in parts by weight, adding the mixture into 50° C. water, controlling the stirring speed at 60 rpm, stirring for 30 min, and fully stirring to obtain a mixed solution B, wherein the anti-corrosion component is prepared by compounding 2-dodecyl imidazoline and sodium nitrite in a mass ratio of 23:20; Step b: adding a filler, a film-forming agent and sodium benzoate to the mixed solution B, controlling the stirring speed to 80 rpm, stirring for 40 minutes, filtering, cooling and packaging in a closed container to obtain a preservative for the surface of a metal material, wherein the filler is composed of diatomaceous earth, kaolin and calcium carbonate in a mass ratio of 1:2:1, the film-forming agent is compounded by a gelatin solution, an alum solution and a glutaraldehyde solution in a mass ratio of 1:2:0.2, the gelatin solution is prepared by adding 80g of gelatin to 1L of water, controlling the water temperature to 60°C, and fully stirring, the alum solution is prepared by adding 20g of alum to 1L of water, and fully stirring at room temperature, and the glutaraldehyde solution is prepared by adding 55g of glutaraldehyde to 1L of water, and fully stirring at room temperature.
[0040] Comparative Example 2 A corrosion inhibitor for the surface of a metal material comprises the following raw materials in parts by weight: 2 parts of an anticorrosive component, 1 part of a modified corrosion inhibitor, 2 parts of a filler, 1 part of a film former, 1 part of an auxiliary agent, and 50 parts of water.
[0041] Wherein, the preparation of the modified corrosion inhibitor comprises the following steps: Step A, preparing a core material solution: dispersing zinc phosphate, sodium molybdate and montmorillonite in a mass ratio of 30:15:18 in water, stirring with a high-speed stirrer, setting the speed to 1000 rpm, stirring at room temperature for 20 minutes, and controlling the mass percentage concentration of the core material solution to be 20%; Step B, preparing a wall material solution: dispersing polyvinyl alcohol, polyvinyl pyrrolidone and polyoxyethylene ether in a mass ratio of 2:1:0.2 in 80°C water, stirring with a high-speed stirrer at a speed of 2000 rpm for 30 minutes, and controlling the mass percentage concentration of the wall material solution to be 10%; Step C, polymerization reaction: adding the core material solution to the wall material solution, controlling the mass ratio of the core material solution to the wall material solution to be 1:2, stirring while adding, controlling the stirring speed to be 300 rpm, stirring for 3 hours, to obtain a mixed solution A; Step D, cross-linking: glutaraldehyde was added to the mixed solution A, stirred at 200 rpm for 5 min, the amount of glutaraldehyde was controlled to be 1% of the total mass of the mixed solution A, and dried at 60° C. until the humidity was 8%, to obtain a modified corrosion inhibitor.
[0042] A method for preparing an anticorrosive agent for the surface of a metal material comprises the following steps: Step a: After mixing the anti-corrosion component and the modified corrosion inhibitor in parts by weight, adding them into 50° C. water, controlling the stirring speed at 60 rpm, stirring for 30 minutes, and fully stirring to obtain a mixed solution B, wherein the anti-corrosion component is prepared by compounding 2-dodecyl imidazoline and benzotriazole in a mass ratio of 18:5; Step b: adding a filler, a film-forming agent and sodium benzoate to the mixed solution B, controlling the stirring speed to 80 rpm, stirring for 40 minutes, filtering, cooling and packaging in a closed container to obtain a preservative for the surface of a metal material, wherein the filler is composed of diatomaceous earth, kaolin and calcium carbonate in a mass ratio of 1:2:1, the film-forming agent is compounded by a gelatin solution, an alum solution and a glutaraldehyde solution in a mass ratio of 1:2:0.2, the gelatin solution is prepared by adding 80g of gelatin to 1L of water, controlling the water temperature to 60°C, and fully stirring, the alum solution is prepared by adding 20g of alum to 1L of water, and fully stirring at room temperature, and the glutaraldehyde solution is prepared by adding 55g of glutaraldehyde to 1L of water, and fully stirring at room temperature.
[0043] Comparative Example 3 A corrosion inhibitor for the surface of a metal material comprises the following raw materials in parts by weight: 2 parts of an anticorrosive component, 1 part of a modified corrosion inhibitor, 2 parts of a filler, 1 part of a film former, 1 part of an auxiliary agent, and 50 parts of water.
[0044] Wherein, the preparation of the modified corrosion inhibitor comprises the following steps: Step A, preparing a core material solution: dispersing zinc phosphate, sodium molybdate and montmorillonite in a mass ratio of 30:15:18 in water, stirring with a high-speed stirrer, setting the speed to 1000 rpm, stirring at room temperature for 20 minutes, and controlling the mass percentage concentration of the core material solution to be 20%; Step B, preparing a wall material solution: dispersing polyvinyl alcohol, polyvinyl pyrrolidone and polyoxyethylene ether in a mass ratio of 2:1:0.2 in 80°C water, stirring with a high-speed stirrer at a speed of 2000 rpm for 30 minutes, and controlling the mass percentage concentration of the wall material solution to be 10%; Step C, polymerization reaction: adding the core material solution to the wall material solution, controlling the mass ratio of the core material solution to the wall material solution to be 1:2, stirring while adding, controlling the stirring speed to be 300 rpm, stirring for 3 hours, to obtain a mixed solution A; Step D, cross-linking: glutaraldehyde was added to the mixed solution A, stirred at 200 rpm for 5 min, the amount of glutaraldehyde was controlled to be 1% of the total mass of the mixed solution A, and dried at 60° C. until the humidity was 8%, to obtain a modified corrosion inhibitor.
[0045] A method for preparing an anticorrosive agent for the surface of a metal material comprises the following steps: Step a: After mixing the anti-corrosion component and the modified corrosion inhibitor in parts by weight, adding them into 50° C. water, controlling the stirring speed at 60 rpm, stirring for 30 minutes, and fully stirring to obtain a mixed solution B, wherein the anti-corrosion component is prepared by compounding sodium nitrite and benzotriazole in a mass ratio of 20:23; Step b: adding a filler, a film-forming agent and sodium benzoate to the mixed solution B, controlling the stirring speed to 80 rpm, stirring for 40 minutes, filtering, cooling and packaging in a closed container to obtain a preservative for the surface of a metal material, wherein the filler is composed of diatomaceous earth, kaolin and calcium carbonate in a mass ratio of 1:2:1, the film-forming agent is compounded by a gelatin solution, an alum solution and a glutaraldehyde solution in a mass ratio of 1:2:0.2, the gelatin solution is prepared by adding 80g of gelatin to 1L of water, controlling the water temperature to 60°C, and fully stirring, the alum solution is prepared by adding 20g of alum to 1L of water, and fully stirring at room temperature, and the glutaraldehyde solution is prepared by adding 55g of glutaraldehyde to 1L of water, and fully stirring at room temperature.
[0046] Comparative Example 4 A corrosion inhibitor for the surface of a metal material comprises the following raw materials in parts by weight: 2 parts of an anticorrosive component, 1 part of a modified corrosion inhibitor, 2 parts of a filler, 1 part of a film former, 1 part of an auxiliary agent, and 50 parts of water.
[0047] Wherein, the preparation of the modified corrosion inhibitor comprises the following steps: Step A, preparing a core material solution: dispersing zinc phosphate and montmorillonite in a mass ratio of 45:18 in water, stirring with a high-speed stirrer, setting the speed to 1000 rpm, stirring at room temperature for 20 minutes, and controlling the mass percentage concentration of the core material solution to be 20%; Step B, preparing a wall material solution: dispersing polyvinyl alcohol, polyvinyl pyrrolidone and polyoxyethylene ether in a mass ratio of 2:1:0.2 in 80°C water, stirring with a high-speed stirrer at a speed of 2000 rpm for 30 minutes, and controlling the mass percentage concentration of the wall material solution to be 10%; Step C, polymerization reaction: adding the core material solution to the wall material solution, controlling the mass ratio of the core material solution to the wall material solution to be 1:2, stirring while adding, controlling the stirring speed to be 300 rpm, stirring for 3 hours, to obtain a mixed solution A; Step D, cross-linking: glutaraldehyde was added to the mixed solution A, stirred at 200 rpm for 5 min, the amount of glutaraldehyde was controlled to be 1% of the total mass of the mixed solution A, and dried at 60° C. until the humidity was 8%, to obtain a modified corrosion inhibitor.
[0048] A method for preparing an anticorrosive agent for the surface of a metal material comprises the following steps: Step a: After mixing the anti-corrosion component and the modified corrosion inhibitor in parts by weight, adding them into 50° C. water, controlling the stirring speed at 60 rpm, stirring for 30 minutes, and fully stirring to obtain a mixed solution B, wherein the anti-corrosion component is prepared by compounding 2-dodecyl imidazoline, sodium nitrite and benzotriazole in a mass ratio of 18:20:5; Step b: adding a filler, a film-forming agent and sodium benzoate to the mixed solution B, controlling the stirring speed to 80 rpm, stirring for 40 minutes, filtering, cooling and packaging in a closed container to obtain a preservative for the surface of a metal material, wherein the filler is composed of diatomaceous earth, kaolin and calcium carbonate in a mass ratio of 1:2:1, the film-forming agent is compounded by a gelatin solution, an alum solution and a glutaraldehyde solution in a mass ratio of 1:2:0.2, the gelatin solution is prepared by adding 80g of gelatin to 1L of water, controlling the water temperature to 60°C, and fully stirring, the alum solution is prepared by adding 20g of alum to 1L of water, and fully stirring at room temperature, and the glutaraldehyde solution is prepared by adding 55g of glutaraldehyde to 1L of water, and fully stirring at room temperature.
[0049] Comparative Example 5 A corrosion inhibitor for the surface of a metal material comprises the following raw materials in parts by weight: 2 parts of an anticorrosive component, 1 part of a modified corrosion inhibitor, 2 parts of a filler, 1 part of a film former, 1 part of an auxiliary agent, and 50 parts of water.
[0050] Wherein, the preparation of the modified corrosion inhibitor comprises the following steps: Step A, preparing a core material solution: dispersing sodium molybdate and montmorillonite in a mass ratio of 45:18 in water, stirring with a high-speed stirrer, setting the speed to 1000 rpm, stirring at room temperature for 20 minutes, and controlling the mass percentage concentration of the core material solution to be 20%; Step B, preparing a wall material solution: dispersing polyvinyl alcohol, polyvinyl pyrrolidone and polyoxyethylene ether in a mass ratio of 2:1:0.2 in 80°C water, stirring with a high-speed stirrer at a speed of 2000 rpm for 30 minutes, and controlling the mass percentage concentration of the wall material solution to be 10%; Step C, polymerization reaction: adding the core material solution to the wall material solution, controlling the mass ratio of the core material solution to the wall material solution to be 1:2, stirring while adding, controlling the stirring speed to be 300 rpm, stirring for 3 hours, to obtain a mixed solution A; Step D, cross-linking: glutaraldehyde was added to the mixed solution A, stirred at 200 rpm for 5 min, the amount of glutaraldehyde was controlled to be 1% of the total mass of the mixed solution A, and dried at 60° C. until the humidity was 8%, to obtain a modified corrosion inhibitor.
[0051] A method for preparing an anticorrosive agent for the surface of a metal material comprises the following steps: Step a: After mixing the anti-corrosion component and the modified corrosion inhibitor in parts by weight, adding them into 50° C. water, controlling the stirring speed at 60 rpm, stirring for 30 minutes, and fully stirring to obtain a mixed solution B, wherein the anti-corrosion component is prepared by compounding 2-dodecyl imidazoline, sodium nitrite and benzotriazole in a mass ratio of 18:20:5; Step b: adding a filler, a film-forming agent and sodium benzoate to the mixed solution B, controlling the stirring speed to 80 rpm, stirring for 40 minutes, filtering, cooling and packaging in a closed container to obtain a preservative for the surface of a metal material, wherein the filler is composed of diatomaceous earth, kaolin and calcium carbonate in a mass ratio of 1:2:1, the film-forming agent is compounded by a gelatin solution, an alum solution and a glutaraldehyde solution in a mass ratio of 1:2:0.2, the gelatin solution is prepared by adding 80g of gelatin to 1L of water, controlling the water temperature to 60°C, and fully stirring, the alum solution is prepared by adding 20g of alum to 1L of water, and fully stirring at room temperature, and the glutaraldehyde solution is prepared by adding 55g of glutaraldehyde to 1L of water, and fully stirring at room temperature.
[0052] Comparative Example 6 A corrosion inhibitor for the surface of a metal material comprises the following raw materials in parts by weight: 2 parts of an anticorrosive component, 1 part of a modified corrosion inhibitor, 2 parts of a filler, 1 part of a film former, 1 part of an auxiliary agent, and 50 parts of water.
[0053] Wherein, the preparation of the modified corrosion inhibitor comprises the following steps: Step A, preparing a core material solution: dispersing zinc phosphate and sodium molybdate in a mass ratio of 30:15 in water, stirring with a high-speed stirrer, setting the speed to 1000 rpm, stirring at room temperature for 20 minutes, and controlling the mass percentage concentration of the core material solution to be 20%; Step B, preparing a wall material solution: dispersing polyvinyl alcohol, polyacrylic acid, polyvinyl pyrrolidone and polyoxyethylene ether in a mass ratio of 2:3:1:0.2 in 80°C water, stirring with a high-speed stirrer at a speed of 2000 rpm for 30 minutes, and controlling the mass percentage concentration of the wall material solution to be 10%; Step C, polymerization reaction: adding the core material solution to the wall material solution, controlling the mass ratio of the core material solution to the wall material solution to be 1:2, stirring while adding, controlling the stirring speed to be 300 rpm, stirring for 3 hours, to obtain a mixed solution A; Step D, cross-linking: glutaraldehyde was added to the mixed solution A, stirred at 200 rpm for 5 min, the amount of glutaraldehyde was controlled to be 1% of the total mass of the mixed solution A, and dried at 60° C. until the humidity was 8%, to obtain a modified corrosion inhibitor.
[0054] A method for preparing an anticorrosive agent for the surface of a metal material comprises the following steps: Step a: After mixing the anti-corrosion component and the modified corrosion inhibitor in parts by weight, adding them into 50° C. water, controlling the stirring speed at 60 rpm, stirring for 30 minutes, and fully stirring to obtain a mixed solution B, wherein the anti-corrosion component is prepared by compounding 2-dodecyl imidazoline, sodium nitrite and benzotriazole in a mass ratio of 18:20:5; Step b: adding a filler, a film-forming agent and sodium benzoate to the mixed solution B, controlling the stirring speed to 80 rpm, stirring for 40 minutes, filtering, cooling and packaging in a closed container to obtain a preservative for the surface of a metal material, wherein the filler is composed of diatomaceous earth, kaolin and calcium carbonate in a mass ratio of 1:2:1, the film-forming agent is compounded by a gelatin solution, an alum solution and a glutaraldehyde solution in a mass ratio of 1:2:0.2, the gelatin solution is prepared by adding 80g of gelatin to 1L of water, controlling the water temperature to 60°C, and fully stirring, the alum solution is prepared by adding 20g of alum to 1L of water, and fully stirring at room temperature, and the glutaraldehyde solution is prepared by adding 55g of glutaraldehyde to 1L of water, and fully stirring at room temperature.
[0055] Comparative Example 7 A corrosion inhibitor for the surface of a metal material comprises the following raw materials in parts by weight: 2 parts of an anticorrosive component, 1 part of a modified corrosion inhibitor, 2 parts of a filler, 1 part of a film former, 1 part of an auxiliary agent, and 50 parts of water.
[0056] Wherein, the preparation of the modified corrosion inhibitor comprises the following steps: Step A, dispersing zinc phosphate, sodium molybdate and montmorillonite in a mass ratio of 30:15:18 in water to obtain a mixed solution A, stirring with a high-speed stirrer, setting the speed to 1000 rpm, stirring at room temperature for 20 minutes, and controlling the mass percentage concentration of the mixed solution A to be 20%; Step B, drying the mixed solution A at 60° C. until the humidity is 8%, thereby obtaining a modified corrosion inhibitor.
[0057] A method for preparing an anticorrosive agent for the surface of a metal material comprises the following steps: Step a: After mixing the anti-corrosion component and the modified corrosion inhibitor in parts by weight, adding them into 50° C. water, controlling the stirring speed at 60 rpm, stirring for 30 minutes, and fully stirring to obtain a mixed solution B, wherein the anti-corrosion component is prepared by compounding 2-dodecyl imidazoline, sodium nitrite and benzotriazole in a mass ratio of 18:20:5; Step b: adding a filler, a film-forming agent and sodium benzoate to the mixed solution B, controlling the stirring speed to 80 rpm, stirring for 40 minutes, filtering, cooling and packaging in a closed container to obtain a preservative for the surface of a metal material, wherein the filler is composed of diatomaceous earth, kaolin and calcium carbonate in a mass ratio of 1:2:1, the film-forming agent is compounded by a gelatin solution, an alum solution and a glutaraldehyde solution in a mass ratio of 1:2:0.2, the gelatin solution is prepared by adding 80g of gelatin to 1L of water, controlling the water temperature to 60°C, and fully stirring, the alum solution is prepared by adding 20g of alum to 1L of water, and fully stirring at room temperature, and the glutaraldehyde solution is prepared by adding 55g of glutaraldehyde to 1L of water, and fully stirring at room temperature.
[0058] Comparative Example 8 A corrosion inhibitor for the surface of a metal material comprises the following raw materials in parts by weight: 2 parts of an anticorrosive component, 1 part of a modified corrosion inhibitor, 2 parts of a filler, 1 part of a film former, 1 part of an auxiliary agent, and 50 parts of water.
[0059] Wherein, the preparation of the modified corrosion inhibitor comprises the following steps: Step A, preparing a core material solution: dispersing zinc phosphate, sodium molybdate and montmorillonite in a mass ratio of 30:15:18 in water, stirring with a high-speed stirrer, setting the speed to 1000 rpm, stirring at room temperature for 20 minutes, and controlling the mass percentage concentration of the core material solution to be 20%; Step B, preparing a wall material solution: dispersing polyvinyl alcohol, polyvinyl pyrrolidone and polyoxyethylene ether in a mass ratio of 2:1:0.2 in 80°C water, stirring with a high-speed stirrer for 30 minutes, setting the speed to 2000 rpm, and controlling the mass percentage concentration of the wall material solution to be 10%; Step C, polymerization reaction: adding the core material solution to the wall material solution, controlling the mass ratio of the core material solution to the wall material solution to be 1:2, stirring while adding, controlling the stirring speed to be 300 rpm, stirring for 3 hours, to obtain a mixed solution A; Step D, cross-linking: glutaraldehyde was added to the mixed solution A, stirred at 200 rpm for 5 min, the amount of glutaraldehyde was controlled to be 1% of the total mass of the mixed solution A, and dried at 60° C. until the humidity was 8%, to obtain a modified corrosion inhibitor.
[0060] A method for preparing an anticorrosive agent for the surface of a metal material comprises the following steps: Step a: After mixing the anti-corrosion component and the modified corrosion inhibitor in parts by weight, adding them into 50° C. water, controlling the stirring speed at 60 rpm, stirring for 30 minutes, and fully stirring to obtain a mixed solution B, wherein the anti-corrosion component is prepared by compounding 2-dodecyl imidazoline, sodium nitrite and benzotriazole in a mass ratio of 18:20:5; Step b: adding a filler, a film-forming agent and sodium benzoate to the mixed solution B, controlling the stirring speed at 80 rpm, stirring for 40 minutes, filtering, cooling and packaging in a closed container to obtain a preservative for the surface of a metal material, wherein the filler is composed of diatomaceous earth, kaolin and calcium carbonate in a mass ratio of 1:2:1, the film-forming agent is compounded by a gelatin solution and an alum solution in a mass ratio of 1:2, the gelatin solution is prepared by adding 80 g of gelatin to 1 L of water, controlling the water temperature to 60°C, and fully stirring, and the alum solution is prepared by adding 20 g of alum to 1 L of water and fully stirring at room temperature.
[0061] Comparative Example 9 A corrosion inhibitor for the surface of a metal material comprises the following raw materials in parts by weight: 2 parts of an anticorrosive component, 1 part of a modified corrosion inhibitor, 2 parts of a filler, 1 part of a film former, 1 part of an auxiliary agent, and 50 parts of water.
[0062] Wherein, the preparation of the modified corrosion inhibitor comprises the following steps: Step A, preparing a core material solution: dispersing zinc phosphate, sodium molybdate and montmorillonite in a mass ratio of 30:15:18 in water, stirring with a high-speed stirrer, setting the speed to 1000 rpm, stirring at room temperature for 20 minutes, and controlling the mass percentage concentration of the core material solution to be 20%; Step B, preparing a wall material solution: dispersing polyvinyl alcohol, polyvinyl pyrrolidone and polyoxyethylene ether in a mass ratio of 2:1:0.2 in 80°C water, stirring with a high-speed stirrer at a speed of 2000 rpm for 30 minutes, and controlling the mass percentage concentration of the wall material solution to be 10%; Step C, polymerization reaction: adding the core material solution to the wall material solution, controlling the mass ratio of the core material solution to the wall material solution to be 1:2, stirring while adding, controlling the stirring speed to be 300 rpm, stirring for 3 hours, to obtain a mixed solution A; Step D, cross-linking: glutaraldehyde was added to the mixed solution A, stirred at 200 rpm for 5 min, the amount of glutaraldehyde was controlled to be 1% of the total mass of the mixed solution A, and dried at 60° C. until the humidity was 8%, to obtain a modified corrosion inhibitor.
[0063] A method for preparing an anticorrosive agent for the surface of a metal material comprises the following steps: Step a: After mixing the anti-corrosion component and the modified corrosion inhibitor in parts by weight, adding them into 50° C. water, controlling the stirring speed at 60 rpm, stirring for 30 minutes, and fully stirring to obtain a mixed solution B, wherein the anti-corrosion component is prepared by compounding 2-dodecyl imidazoline, sodium nitrite and benzotriazole in a mass ratio of 18:20:5; Step b: adding a filler, a film-forming agent and sodium benzoate to the mixed solution B, controlling the stirring speed at 80 rpm, stirring for 40 minutes, filtering, cooling and packaging in a closed container to obtain a preservative for the surface of a metal material, wherein the filler is composed of diatomaceous earth, kaolin and calcium carbonate in a mass ratio of 1:2:1, the film-forming agent is compounded from a gelatin solution, an alum solution and a glutaraldehyde solution in a mass ratio of 1:2:0.2, the gelatin solution is prepared by adding 80 g of gelatin to 1 L of water, controlling the water temperature to 60°C and fully stirring, the alum solution is prepared by adding 20 g of alum to 1 L of water and fully stirring at room temperature, and the glutaraldehyde solution is prepared by adding 55 g of glutaraldehyde to 1 L of water and fully stirring at room temperature.
[0064] The comprehensive properties of the anticorrosive agents for metal material surfaces prepared in Examples 1-3 and Comparative Examples 1-9 of the present application are as follows: Adhesion test: Tested in accordance with national standard GB / T 5210-2006; Neutral salt spray resistance test: Tested in accordance with national standard GB / T 1771-2007; Water resistance test: Tested in accordance with national standard GB / T 1733-1993; Corrosion resistance test: Tested in accordance with national standard GB / T 9274-1988; The specific test results are shown in Tables 1 and 2 below.
[0065] Table 1 Performance parameters of preservatives in Examples 1-3
[0066] Table 2 Performance parameters of preservatives in Comparative Examples 1-9
[0067] The present application discloses a preservative for the surface of a metal material. As can be seen from Tables 1 and 2, the preservative prepared in the present application has extremely strong adhesion, and performs outstandingly in terms of water resistance, acid resistance, alkali resistance, and neutral salt spray resistance, and can provide long-term protection for metals, solving the problems of the prior art that cracks, peeling, and poor anti-corrosion effects are easily generated.
[0068] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A corrosion inhibitor for the surface of metal materials, It is characterized in that The antiseptic comprises the following raw materials in parts by weight: 2-5 parts of antiseptic components, 1-2 parts of modified corrosion inhibitors, 2-3 parts of fillers, 1-1.5 parts of film formers, 1-2 parts of additives, and 50-60 parts of water.
2. The anticorrosive agent for the surface of a metal material according to claim 1, It is characterized in that The antiseptic component is prepared by compounding an imidazoline derivative, sodium nitrite and benzotriazole in a mass ratio of 18-20:20-25:5-8.
3. The anticorrosive agent for the surface of a metal material according to claim 1, It is characterized in that The preparation of the modified corrosion inhibitor comprises the following steps: Step A, preparing a core material solution: dispersing zinc phosphate, sodium molybdate and montmorillonite in water; Step B, preparing a wall material solution: dispersing polyvinyl alcohol, polyvinyl pyrrolidone and an emulsifier in 80-90° C. water; Step C, polymerization reaction: adding the core material solution to the wall material solution, stirring while adding, for 3-5 hours, to obtain a mixed solution A; Step D, cross-linking: add a cross-linking agent to the mixed solution A, dry at 60-80° C. until the humidity is less than 10%, to obtain a modified corrosion inhibitor.
4. The anticorrosive agent for the surface of a metal material according to claim 3, It is characterized in that In the step A, the mass ratio of zinc phosphate, sodium molybdate and montmorillonite is 30-40:15-20:18-22.
5. The anticorrosive agent for the surface of a metal material according to claim 3, It is characterized in that In the step B, the mass ratio of polyvinyl alcohol, polyvinyl pyrrolidone and emulsifier is 2-3:1-2:0.2-0.
5.
6. The anticorrosive agent for the surface of a metal material according to claim 3, It is characterized in that In the step C, the mass ratio of the core material solution to the wall material solution is 1-1.5:2-3.
7. The anticorrosive agent for the surface of a metal material according to claim 1, It is characterized in that The filler consists of diatomaceous earth, kaolin and calcium carbonate in a mass ratio of 1-2:2-4:1-3.
8. The anticorrosive agent for the surface of a metal material according to claim 1, It is characterized in that The film-forming agent is prepared by compounding a gelatin solution, an alum solution and a glutaraldehyde solution in a mass ratio of 1-2:2-3:0.2-0.
3.
9. The anticorrosive agent for the surface of a metal material according to claim 8, It is characterized in that The mass percentage concentration of the gelatin solution is 8-10%, the mass percentage concentration of the alum solution is 2-3%, and the mass percentage concentration of the glutaraldehyde solution is 5.5-6%.
10. An anticorrosive agent for the surface of a metal material according to any one of claims 1 to 9, It is characterized in that The specific preparation steps are as follows: Step a: After mixing the anticorrosive component and the modified corrosion inhibitor according to weight parts, add them into 50-60°C water, control the stirring speed to 60-80rpm, stir for 30-40min, and stir thoroughly to obtain a mixed solution B; Step b: Add filler, film-forming agent and auxiliary agent to mixed solution B, control the stirring speed to 80-100 rpm, stir for 40-60 min, filter, cool and package in a sealed container to obtain the preservative for the surface of metal materials.
Citation Information
Patent Citations
Microencapsulated vapor phase rust inhibitor and preparation method thereof
CN104388944A
Silane corrosion resistant film on aluminum alloy surface in ocean environment and preparation method thereof
CN108677178A
Rust-proof paint
CN108864834A
Anticorrosive paint of excrement discharging pipeline and preparation method of anticorrosive paint
CN110305565A
Coating preparation method based on fluorescence induction corrosion
CN118580746A
Cited By
Modified montmorillonite and preparation method thereof, composition for acid-base-resistant modified asphalt, acid-base-resistant modified asphalt and preparation method thereof, and acid-base-resistant asphalt-based waterproof coiled material