High-strength wear-resistant laser leather transfer film and preparation method thereof
By using wear-resistant coatings of silicon nitride, nanodiamond, heavy calcium carbonate, glass fiber and modified acrylic resin in laser leather transfer film, the problem of insufficient wear resistance in the prior art is solved, and high strength wear resistance is achieved The laser leather transfer film is prepared to meet the high wear resistance requirements of modern leather products.
Patent Information
- Application Number
- CN202410952579.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-08
AI Technical Summary
The existing laser leather transfer film has shortcomings in wear resistance, which is difficult to meet the high requirements of modern leather products for wear resistance and use resistance.
Wear-resistant coatings composed of silicon nitride, nanodiamond, heavy calcium carbonate, glass fiber and modified acrylic resin are formed by heating, melting and drying, combining UV release layer, molded color layer, plating and transfer The adhesive layer enhances the wear resistance of the transfer film.
The wear resistance of the laser leather transfer film is significantly improved, the dispersion and compatibility of the filler is increased, and it is difficult to peel, has high hardness and is extremely lubricating, thereby preparing a high-strength wear-resistant laser leather transfer film.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of transfer films and relates to a high-strength and wear-resistant laser leather transfer film and a preparation method thereof. Background Art
[0002] Leather has been loved by people for thousands of years, but early leather has always been brown and black, with very simple colors and types. As people's demand for leather fashion and pursuit of leather products become more prominent, they not only require perfection in color, color, and leather, but also have higher requirements for wear resistance and durability. This is the combination of modern fashion and reality, so the market demand for leather post-processing products such as leather printing is also increasing, and the use of leather transfer film is becoming more and more extensive.
[0003] Chinese patent CN114290846A provides a high-brightness, high-wear-resistant laser leather transfer film and its preparation method. The laser leather transfer film includes a base film and a release layer, a brightening and wear-resistant layer, a molded color layer, a coating and a transfer adhesive layer stacked on the base film in sequence. The brightening and wear-resistant layer is selected from acrylic modified silicone resin. The invention is made of high-hydroxyl value acrylic resin, isocyanate curing agent and a small amount of epoxy curing agent. The high hydroxyl value can increase the degree of cross-linking with the curing agent and increase wear resistance. At the same time, the refractive index and light transmittance of high-hydroxyl value acrylic resin are also higher than those of low hydroxyl value, and it is easier to reflect the brightness of the aluminum plating layer. In addition, high hydroxyl value acrylic resin can enhance the adhesion between the brightening and wear-resistant layer and the coating. Therefore, the high-strength and wear-resistant laser leather transfer film provided by the present invention on this basis can further improve its wear resistance. Summary of the invention
[0004] The present invention relates to a high-strength and wear-resistant laser leather transfer film and a preparation method thereof, and belongs to the technical field of transfer films. The present invention discloses a high-strength and wear-resistant laser leather transfer film, wherein a release layer, a wear-resistant layer, a molded color layer, a plating layer and a transfer adhesive layer are stacked on a base film. The wear-resistant layer is composed of silicon nitride, nano-diamonds, heavy calcium carbonate, glass fiber and modified acrylic resin, and the dispersion and compatibility of the filler are further increased by carboxyl modification of the acrylic resin; the addition of silicon nitride, nano-diamonds, heavy calcium carbonate and glass fiber greatly enhances the wear resistance of the transfer film in terms of being difficult to peel off, high hardness and extremely lubricating. Therefore, the present invention can prepare a high-strength and wear-resistant laser leather transfer film.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] A high-strength wear-resistant laser leather transfer film, which takes a base film as the bottom, and is sequentially coated with a release layer, a wear-resistant layer, a molded color layer, a plating layer and a transfer adhesive layer, wherein the wear-resistant layer is made of a wear-resistant coating that is heated and melted, coated and dried, and the wear-resistant coating is composed of silicon nitride, nano-diamond, heavy calcium carbonate, glass fiber and modified acrylic resin.
[0007] Furthermore, the mass ratio of the silicon nitride, nano-diamond, heavy calcium carbonate, glass fiber and modified acrylic resin is 1-3:2-3:1-3:2:20-50, and the preparation method of the modified acrylic resin comprises the following steps:
[0008] A1: Toluene is heated and then a mixture of methyl methacrylate, n-butyl acrylate, hydroxyethyl acrylate and azobisisobutyronitrile is added, followed by heat preservation to obtain a pretreated acrylic resin;
[0009] A2: The pretreated acrylic resin is heated continuously, and a catalyst and succinic anhydride are added and stirred to form a mixture a, and then petroleum ether is added for precipitation, and the petroleum ether is filtered and recovered, and then vacuum dried to form a primary acrylic resin;
[0010] A3: Initially, the acrylic resin is heated, a catalyst and glutaric anhydride are added, stirred and mixed to form a mixture b, petroleum ether is added for precipitation, the petroleum ether is recovered by filtration, and then vacuum dried to obtain a modified acrylic resin.
[0011] Furthermore, in the step A1, the temperature of heating toluene is 85-90° C., the mass ratio of toluene, methyl methacrylate, n-butyl acrylate, hydroxyethyl acrylate and azobisisobutyronitrile is 10:6-7:2:1.2-1.3:0.2, and the insulation time is 1-1.5 h.
[0012] Furthermore, the heating temperature in step A2 is 110-120° C., the mass ratio of the pretreated acrylic resin, the catalyst and succinic anhydride is 20-30:0.01-0.02:0.8-1, the stirring time is 40-60 min, the mass ratio of the mixture a to petroleum ether is 1-5:3, and the temperature and time of the vacuum drying are 40° C. and 30-40 min, respectively.
[0013] Furthermore, in the step A3, the temperature at which the initial acrylic resin is heated is 110-120° C., the mass ratio of the initial acrylic resin, the catalyst and glutaric anhydride is 20-30:0.01-0.02:1-1.2, the stirring and mixing time is 40-60 min, the mass ratio of the mixture b to petroleum ether is 2-3:6, the temperature and time of the vacuum drying are 40° C. and 30-40 min, respectively, and the catalyst in the steps A2 and 3 is p-toluenesulfonic acid.
[0014] Furthermore, the thicknesses of the release layer, wear-resistant layer, molded color layer, plating layer and transfer adhesive layer are 1-2μm, 1-3μm, 1-2μm, 50-200nm and 1-5μm respectively. The molded color layer is obtained by drying the color layer coating by a molding machine and then molding it, wherein the color layer coating is composed of high-hydroxy acrylic resin, isocyanate curing agent, epoxy curing agent, color powder, dispersant and solvent in a mass ratio of 100:3-5:0.5-1:2-5:0.5-2:150-200.
[0015] Furthermore, the transfer adhesive layer is formed by coating with transfer adhesive composed of styrene thermoplastic elastomer, epoxy resin, thiol curing agent and solvent in a mass ratio of 100:15:5-8:150-200 and drying.
[0016] Furthermore, the preparation method of the high-strength and wear-resistant laser leather transfer film comprises the following steps:
[0017] (1) firstly coating a UV release agent on the surface of the base film and irradiating the base film with UV light to form a release layer;
[0018] (2) then applying a heated and melted wear-resistant coating on the surface of the release layer and drying it to form a wear-resistant layer;
[0019] (3) coating a color layer coating on the surface of the wear-resistant layer, drying it to form a color layer, and then using a molding machine to mold the color layer to form a molded color layer, and then vacuum plating the surface to form an aluminum plating layer;
[0020] (4) The coating surface is coated with transfer glue, which is dried to form a transfer glue layer, and then aged at 45° C. for 48 h. After cooling, a high-strength and wear-resistant laser leather transfer film is obtained.
[0021] Beneficial effects of the present invention:
[0022] 1. The present invention further increases the dispersibility and compatibility of fillers by carboxylating acrylic resin; adding silicon nitride, nano-diamond, heavy calcium carbonate and glass fiber as fillers greatly enhances the wear resistance of the transfer film from the aspects of difficult peeling, high hardness and high lubricity. Therefore, the present invention can prepare a high-strength and wear-resistant laser leather transfer film. DETAILED DESCRIPTION
[0023] In order to further illustrate the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention are described in detail below in combination with embodiments.
[0024] Example 1
[0025] A high-strength wear-resistant laser leather transfer film, which takes a base film as the bottom, and is sequentially coated with a release layer, a wear-resistant layer, a molded color layer, a plating layer and a transfer adhesive layer, wherein the wear-resistant layer is made of a wear-resistant coating that is heated and melted, coated and dried, and the wear-resistant coating is composed of silicon nitride, nano-diamond, heavy calcium carbonate, glass fiber and modified acrylic resin.
[0026] The mass ratio of the silicon nitride, nano-diamond, heavy calcium carbonate, glass fiber and modified acrylic resin is 1:2:1:2:20. The preparation method of the modified acrylic resin comprises the following steps:
[0027] A1: Toluene is heated and then a mixture of methyl methacrylate, n-butyl acrylate, hydroxyethyl acrylate and azobisisobutyronitrile is added, followed by heat preservation to obtain a pretreated acrylic resin;
[0028] A2: The pretreated acrylic resin is heated continuously, and a catalyst and succinic anhydride are added and stirred to form a mixture a, and then petroleum ether is added for precipitation, and the petroleum ether is filtered and recovered, and then vacuum dried to form a primary acrylic resin;
[0029] A3: Initially, the acrylic resin is heated, a catalyst and glutaric anhydride are added, stirred and mixed to form a mixture b, petroleum ether is added for precipitation, the petroleum ether is recovered by filtration, and then vacuum dried to obtain a modified acrylic resin.
[0030] In the step A1, the temperature at which toluene is heated is 85° C., the mass ratio of toluene, methyl methacrylate, n-butyl acrylate, hydroxyethyl acrylate, and azobisisobutyronitrile is 10:6:2:1.2:0.2, and the insulation time is 1 hour.
[0031] The heating temperature in step A2 is 110° C., the mass ratio of the pretreated acrylic resin, the catalyst and succinic anhydride is 20:0.01:0.8, the stirring time is 40 min, the mass ratio of the mixture a to petroleum ether is 1:3, and the temperature and time of the vacuum drying are 40° C. and 30 min, respectively.
[0032] The temperature of heating the primary acrylic resin in step A3 is 110° C., the mass ratio of the primary acrylic resin, the catalyst and glutaric anhydride is 20:0.01:1, the stirring and mixing time is 40 min, the mass ratio of the mixture b to petroleum ether is 2:6, the temperature and time of vacuum drying are 40° C. and 30 min respectively, and the catalyst in steps A2 and 3 is p-toluenesulfonic acid.
[0033] The thicknesses of the release layer, wear-resistant layer, molded color layer, plating layer and transfer adhesive layer are 1μm, 1μm, 1μm, 50nm and 1μm respectively. The molded color layer is obtained by drying the color layer coating on a molding machine and then molding it. The color layer coating consists of high-hydroxy acrylic resin, isocyanate curing agent, epoxy curing agent, color powder, dispersant and solvent in a mass ratio of 100:3:0.5:2:0.5:150.
[0034] The transfer adhesive layer is formed by coating with transfer adhesive composed of styrene thermoplastic elastomer, epoxy resin, thiol curing agent and solvent in a mass ratio of 100:15:5:150 and drying.
[0035] The preparation method of the high-strength wear-resistant laser leather transfer film comprises the following steps:
[0036] (1) firstly coating a UV release agent on the surface of the base film and irradiating the base film with UV light to form a release layer;
[0037] (2) then applying a heated and melted wear-resistant coating on the surface of the release layer and drying it to form a wear-resistant layer;
[0038] (3) coating a color layer coating on the surface of the wear-resistant layer, drying it to form a color layer, and then using a molding machine to mold the color layer to form a molded color layer, and then vacuum plating the surface to form an aluminum plating layer;
[0039] (4) The coating surface is coated with transfer glue, which is dried to form a transfer glue layer, and then aged at 45° C. for 48 h. After cooling, a high-strength and wear-resistant laser leather transfer film is obtained.
[0040] The purchase source of the nano diamond couple: Nano Diamond / Zhongke Leiming-7782-40-3, the purchase source of heavy calcium carbonate: Heavy calcium carbonate / Qingjiang, the purchase source of p-toluenesulfonic acid: p-toluenesulfonic acid / Lianfeng-104-15-4, the purchase source of high hydroxyl acrylic resin: High hydroxyl acrylic resin / Jinfengyuan-RS-7030F, the purchase source of isocyanate curing agent: Isocyanate curing agent / Evonik-VESTAGON BF-1540, Source of purchase of epoxy curing agent: epoxy curing agent / Runfeng Synthetic Technology-1477-55-0, Source of purchase of toner: toner / Quanfeng, Source of purchase of dispersant: dispersant / EBS-QY2024, the solvent is toluene, Source of purchase of styrene thermoplastic elastomer: styrene thermoplastic elastomer / BYK-BYK-8112FA, Source of purchase of epoxy resin: epoxy resin / OLIN-DER331, Source of purchase of thiol curing agent: thiol curing agent / Phillips, USA-7773-83-3, Source of purchase of UV release agent: UV release agent / LENCOLO-Lencolo 8769.
[0041] Example 2
[0042] A high-strength wear-resistant laser leather transfer film, which takes a base film as the bottom, and is sequentially coated with a release layer, a wear-resistant layer, a molded color layer, a plating layer and a transfer adhesive layer, wherein the wear-resistant layer is made of a wear-resistant coating that is heated and melted, coated and dried, and the wear-resistant coating is composed of silicon nitride, nano-diamond, heavy calcium carbonate, glass fiber and modified acrylic resin.
[0043] The mass ratio of the silicon nitride, nano-diamond, heavy calcium carbonate, glass fiber and modified acrylic resin is 2:2.5:2:2:35. The preparation method of the modified acrylic resin comprises the following steps:
[0044] A1: Toluene is heated and then a mixture of methyl methacrylate, n-butyl acrylate, hydroxyethyl acrylate and azobisisobutyronitrile is added, followed by heat preservation to obtain a pretreated acrylic resin;
[0045] A2: The pretreated acrylic resin is heated continuously, and a catalyst and succinic anhydride are added and stirred to form a mixture a, and then petroleum ether is added for precipitation, and the petroleum ether is filtered and recovered, and then vacuum dried to form a primary acrylic resin;
[0046] A3: Initially, the acrylic resin is heated, a catalyst and glutaric anhydride are added, stirred and mixed to form a mixture b, petroleum ether is added for precipitation, the petroleum ether is recovered by filtration, and then vacuum dried to obtain a modified acrylic resin.
[0047] In the step A1, the temperature at which toluene is heated is 88° C., the mass ratio of toluene, methyl methacrylate, n-butyl acrylate, hydroxyethyl acrylate, and azobisisobutyronitrile is 10:6.5:2:1.2:0.2, and the insulation time is 1.2 h.
[0048] The heating temperature in step A2 is 115° C., the mass ratio of the pretreated acrylic resin, the catalyst and succinic anhydride is 25:0.01:0.9, the stirring time is 50 min, the mass ratio of the mixture a to petroleum ether is 1:1, and the temperature and time of the vacuum drying are 40° C. and 35 min, respectively.
[0049] The temperature of heating the primary acrylic resin in step A3 is 115° C., the mass ratio of the primary acrylic resin, the catalyst and glutaric anhydride is 25:0.01:1.1, the stirring and mixing time is 50 min, the mass ratio of the mixture b to petroleum ether is 2.5:6, the temperature and time of vacuum drying are 40° C. and 35 min respectively, and the catalyst in steps A2 and 3 is p-toluenesulfonic acid.
[0050] The thicknesses of the release layer, wear-resistant layer, molded color layer, plating layer and transfer adhesive layer are 1.5μm, 2μm, 1.5μm, 120nm and 3μm respectively. The molded color layer is obtained by drying the color layer coating with a molding machine and then molding it. The color layer coating consists of high-hydroxy acrylic resin, isocyanate curing agent, epoxy curing agent, color powder, dispersant and solvent in a mass ratio of 100:4:0.8:3.5:1.2:180.
[0051] The transfer adhesive layer is formed by coating with transfer adhesive composed of styrene thermoplastic elastomer, epoxy resin, thiol curing agent and solvent in a mass ratio of 100:15:6.5:180 and drying.
[0052] The preparation method of the high-strength wear-resistant laser leather transfer film comprises the following steps:
[0053] (1) firstly coating a UV release agent on the surface of the base film and irradiating the base film with UV light to form a release layer;
[0054] (2) then applying a heated and melted wear-resistant coating on the surface of the release layer and drying it to form a wear-resistant layer;
[0055] (3) coating a color layer coating on the surface of the wear-resistant layer, drying it to form a color layer, and then using a molding machine to mold the color layer to form a molded color layer, and then vacuum plating the surface to form an aluminum plating layer;
[0056] (4) The coating surface is coated with transfer glue, which is dried to form a transfer glue layer, and then aged at 45° C. for 48 h. After cooling, a high-strength and wear-resistant laser leather transfer film is obtained.
[0057] The purchase source of the nano diamond couple: Nano Diamond / Zhongke Leiming-7782-40-3, the purchase source of heavy calcium carbonate: Heavy calcium carbonate / Qingjiang, the purchase source of p-toluenesulfonic acid: p-toluenesulfonic acid / Lianfeng-104-15-4, the purchase source of high hydroxyl acrylic resin: High hydroxyl acrylic resin / Jinfengyuan-RS-7030F, the purchase source of isocyanate curing agent: Isocyanate curing agent / Evonik-VESTAGON BF-1540, Source of purchase of epoxy curing agent: epoxy curing agent / Runfeng Synthetic Technology-1477-55-0, Source of purchase of toner: toner / Quanfeng, Source of purchase of dispersant: dispersant / EBS-QY2024, the solvent is toluene, Source of purchase of styrene thermoplastic elastomer: styrene thermoplastic elastomer / BYK-BYK-8112FA, Source of purchase of epoxy resin: epoxy resin / OLIN-DER331, Source of purchase of thiol curing agent: thiol curing agent / Phillips, USA-7773-83-3, Source of purchase of UV release agent: UV release agent / LENCOLO-Lencolo 8769.
[0058] Example 3
[0059] A high-strength wear-resistant laser leather transfer film, which takes a base film as the bottom, and is sequentially coated with a release layer, a wear-resistant layer, a molded color layer, a plating layer and a transfer adhesive layer, wherein the wear-resistant layer is made of a wear-resistant coating that is heated and melted, coated and dried, and the wear-resistant coating is composed of silicon nitride, nano-diamond, heavy calcium carbonate, glass fiber and modified acrylic resin.
[0060] The mass ratio of the silicon nitride, nano-diamond, heavy calcium carbonate, glass fiber and modified acrylic resin is 3:3:3:2:50. The preparation method of the modified acrylic resin comprises the following steps:
[0061] A1: Toluene is heated and then a mixture of methyl methacrylate, n-butyl acrylate, hydroxyethyl acrylate and azobisisobutyronitrile is added, followed by heat preservation to obtain a pretreated acrylic resin;
[0062] A2: The pretreated acrylic resin is heated continuously, and a catalyst and succinic anhydride are added and stirred to form a mixture a, and then petroleum ether is added for precipitation, and the petroleum ether is filtered and recovered, and then vacuum dried to form a primary acrylic resin;
[0063] A3: Initially, the acrylic resin is heated, a catalyst and glutaric anhydride are added, stirred and mixed to form a mixture b, petroleum ether is added for precipitation, the petroleum ether is recovered by filtration, and then vacuum dried to obtain a modified acrylic resin.
[0064] In the step A1, the temperature at which toluene is heated is 90° C., the mass ratio of toluene, methyl methacrylate, n-butyl acrylate, hydroxyethyl acrylate, and azobisisobutyronitrile is 10:7:2:1.3:0.2, and the insulation time is 1.5 h.
[0065] The heating temperature in step A2 is 120° C., the mass ratio of the pretreated acrylic resin, the catalyst and succinic anhydride is 30:0.02:1, the stirring time is 60 min, the mass ratio of the mixture a to petroleum ether is 5:3, and the temperature and time of the vacuum drying are 40° C. and 40 min, respectively.
[0066] The temperature of heating the primary acrylic resin in step A3 is 120° C., the mass ratio of the primary acrylic resin, the catalyst and glutaric anhydride is 30:0.02:1.2, the stirring and mixing time is 60 min, the mass ratio of the mixture b to petroleum ether is 3:6, the temperature and time of vacuum drying are 40° C. and 40 min respectively, and the catalyst in steps A2 and 3 is p-toluenesulfonic acid.
[0067] The thicknesses of the release layer, wear-resistant layer, molded color layer, plating layer and transfer adhesive layer are 2μm, 3μm, 2μm, 200nm and 5μm respectively. The molded color layer is obtained by drying the color layer coating by a molding machine and then molding it. The color layer coating consists of high-hydroxy acrylic resin, isocyanate curing agent, epoxy curing agent, color powder, dispersant and solvent in a mass ratio of 100:5:1:5:2:200.
[0068] The transfer adhesive layer is formed by coating with transfer adhesive composed of styrene thermoplastic elastomer, epoxy resin, thiol curing agent and solvent in a mass ratio of 100:15:8:200 and drying.
[0069] The preparation method of the high-strength wear-resistant laser leather transfer film comprises the following steps:
[0070] (1) firstly coating a UV release agent on the surface of the base film and irradiating the base film with UV light to form a release layer;
[0071] (2) then applying a heated and melted wear-resistant coating on the surface of the release layer and drying it to form a wear-resistant layer;
[0072] (3) coating a color layer coating on the surface of the wear-resistant layer, drying it to form a color layer, and then using a molding machine to mold the color layer to form a molded color layer, and then vacuum plating the surface to form an aluminum plating layer;
[0073] (4) The coating surface is coated with transfer glue, which is dried to form a transfer glue layer, and then aged at 45° C. for 48 h. After cooling, a high-strength and wear-resistant laser leather transfer film is obtained.
[0074] The purchase source of the nano diamond couple: Nano Diamond / Zhongke Leiming-7782-40-3, the purchase source of heavy calcium carbonate: Heavy calcium carbonate / Qingjiang, the purchase source of p-toluenesulfonic acid: p-toluenesulfonic acid / Lianfeng-104-15-4, the purchase source of high hydroxyl acrylic resin: High hydroxyl acrylic resin / Jinfengyuan-RS-7030F, the purchase source of isocyanate curing agent: Isocyanate curing agent / Evonik-VESTAGON BF-1540, Source of purchase of epoxy curing agent: epoxy curing agent / Runfeng Synthetic Technology-1477-55-0, Source of purchase of toner: toner / Quanfeng, Source of purchase of dispersant: dispersant / EBS-QY2024, the solvent is toluene, Source of purchase of styrene thermoplastic elastomer: styrene thermoplastic elastomer / BYK-BYK-8112FA, Source of purchase of epoxy resin: epoxy resin / OLIN-DER331, Source of purchase of thiol curing agent: thiol curing agent / Phillips, USA-7773-83-3, Source of purchase of UV release agent: UV release agent / LENCOLO-Lencolo 8769.
[0075] Comparative Example 1
[0076] On the basis of Example 2, the silicon nitride in the wear-resistant coating is removed and replaced with nano-diamond of equal mass, and other conditions are consistent with Example 2.
[0077] Comparative Example 2
[0078] On the basis of Example 2, the nano-diamond in the wear-resistant coating is removed and replaced with silicon nitride of equal mass, and other conditions are consistent with Example 2.
[0079] Comparative Example 3
[0080] On the basis of Example 2, the heavy calcium carbonate in the wear-resistant coating was removed and replaced with nano-diamonds of equal mass, and other conditions were consistent with Example 2.
[0081] Comparative Example 4
[0082] On the basis of Example 2, the glass fiber in the wear-resistant coating is removed and replaced with an equal mass of heavy calcium carbonate. Other conditions are consistent with Example 2.
[0083] Comparative Example 5
[0084] On the basis of Example 2, a high-strength and wear-resistant laser leather transfer film is provided. The high-strength and wear-resistant laser leather transfer film is based on a base film, and is sequentially coated with a release layer, a wear-resistant layer, a molded color layer, a plating layer and a transfer adhesive layer, wherein the wear-resistant layer is made of a wear-resistant coating that is heated and melted, coated and dried, and the wear-resistant coating is composed of silicon nitride, nano-diamond, heavy calcium carbonate, glass fiber and acrylic resin.
[0085] The mass ratio of the silicon nitride, nano-diamond, heavy calcium carbonate, glass fiber and acrylic resin is 2:2.5:2:2:35. The preparation method of the acrylic resin comprises the following steps:
[0086] A1: Heat toluene and then add a mixture of methyl methacrylate, n-butyl acrylate, hydroxyethyl acrylate and azobisisobutyronitrile, and then keep warm to obtain acrylic resin;
[0087] In the step A1, the temperature at which toluene is heated is 88° C., the mass ratio of toluene, methyl methacrylate, n-butyl acrylate, hydroxyethyl acrylate, and azobisisobutyronitrile is 10:6.5:2:1.2:0.2, and the insulation time is 1.2 h.
[0088] The thicknesses of the release layer, wear-resistant layer, molded color layer, plating layer and transfer adhesive layer are 1.5μm, 2μm, 1.5μm, 120nm and 3μm respectively. The molded color layer is obtained by drying the color layer coating with a molding machine and then molding it. The color layer coating consists of high-hydroxy acrylic resin, isocyanate curing agent, epoxy curing agent, color powder, dispersant and solvent in a mass ratio of 100:4:0.8:3.5:1.2:180.
[0089] The transfer adhesive layer is formed by coating with transfer adhesive composed of styrene thermoplastic elastomer, epoxy resin, thiol curing agent and solvent in a mass ratio of 100:15:6.5:180 and drying.
[0090] The preparation method of the high-strength wear-resistant laser leather transfer film comprises the following steps:
[0091] (1) firstly coating a UV release agent on the surface of the base film and irradiating the base film with UV light to form a release layer;
[0092] (2) then applying a heated and melted wear-resistant coating on the surface of the release layer and drying it to form a wear-resistant layer;
[0093] (3) coating a color layer coating on the surface of the wear-resistant layer, drying it to form a color layer, and then using a molding machine to mold the color layer to form a molded color layer, and then vacuum plating the surface to form an aluminum plating layer;
[0094] (4) The coating surface is coated with transfer glue, which is dried to form a transfer glue layer, and then aged at 45° C. for 48 h. After cooling, a high-strength and wear-resistant laser leather transfer film is obtained.
[0095] 1. Performance Testing
[0096] According to the paint film wear resistance determination method of GBT 1768-1979, the wear resistance test of Example 2 and Comparative Examples 1-5 was carried out. The test results are shown in Table 1.
[0097] Table 1 Test results
[0098] Sample Wear resistance grade Example 2 Level 5 Comparative Example 1 Level 3 Comparative Example 2 Level 3 Comparative Example 3 Level 3 Comparative Example 4 Level 3 Comparative Example 5 Level 2
[0099] It can be seen from Table 1 that the wear resistance level of Example 2 is greater than that of Comparative Examples 1-5, that is, the wear resistance of Example 2 is greater than that of Comparative Examples 1-5. In Comparative Examples 1-4, one of silicon nitride, nano-diamond, heavy calcium carbonate, and glass fiber is removed, and the wear resistance is significantly reduced. Since silicon nitride, nano-diamond, heavy calcium carbonate, and glass fiber have a synergistic effect, the wear resistance of the transfer film is enhanced in terms of being difficult to peel off, high hardness, and excellent lubricity. In Comparative Example 5, the acrylic resin is not modified, and its compatibility with fillers is worse than that of Example 2, so the wear resistance is reduced.
[0100] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.
Claims
1. A high-strength and wear-resistant laser leather transfer film, characterized in that: The high-strength wear-resistant laser leather transfer film is based on a base film, and is sequentially coated with a release layer, a wear-resistant layer, a molded color layer, a plating layer and a transfer adhesive layer, wherein the wear-resistant layer is made of a wear-resistant coating that is heated and melted, coated and dried, and the wear-resistant coating is composed of silicon nitride, nano-diamond, heavy calcium carbonate, glass fiber and modified acrylic resin.
2. The high-strength and wear-resistant laser leather transfer film according to claim 1, characterized in that: The mass ratio of the silicon nitride, nano-diamond, heavy calcium carbonate, glass fiber and modified acrylic resin is 1-3:2-3:1-3:2:20-50. The preparation method of the modified acrylic resin comprises the following steps: A1: After heating toluene, a mixture of methyl methacrylate, n-butyl acrylate, hydroxyethyl acrylate and azobisisobutyronitrile is added, followed by heat preservation to obtain a pretreated acrylic resin; A2: The pretreated acrylic resin is heated continuously, and a catalyst and succinic anhydride are added and stirred to form a mixture a, and then petroleum ether is added for precipitation, and the petroleum ether is filtered and recovered, and then vacuum dried to form a primary acrylic resin; A3: Initially, the acrylic resin is heated, a catalyst and glutaric anhydride are added, stirred and mixed to form a mixture b, petroleum ether is added for precipitation, the petroleum ether is recovered by filtration, and then vacuum dried to obtain a modified acrylic resin.
3. The high-strength and wear-resistant laser leather transfer film according to claim 2, characterized in that: In the step A1, the temperature at which toluene is heated is 85-90° C., the mass ratio of toluene, methyl methacrylate, n-butyl acrylate, hydroxyethyl acrylate and azobisisobutyronitrile is 10:6-7:2:1.2-1.3:0.2, and the insulation time is 1-1.5 h.
4. The high-strength and wear-resistant laser leather transfer film according to claim 2, characterized in that: The heating temperature in step A2 is 110-120° C., the mass ratio of the pretreated acrylic resin, the catalyst and succinic anhydride is 20-30:0.01-0.02:0.8-1, the stirring time is 40-60 min, the mass ratio of the mixture a to petroleum ether is 1-5:3, and the temperature and time of the vacuum drying are 40° C. and 30-40 min, respectively.
5. The high-strength and wear-resistant laser leather transfer film according to claim 2, characterized in that: The temperature of heating the primary acrylic resin in step A3 is 110-120°C, the mass ratio of the primary acrylic resin, the catalyst and glutaric anhydride is 20-30:0.01-0.02:1-1.2, the stirring and mixing time is 40-60min, the mass ratio of the mixture b to petroleum ether is 2-3:6, the temperature and time of vacuum drying are 40°C and 30-40min respectively, and the catalyst in steps A2 and 3 is p-toluenesulfonic acid.
6. The high-strength and wear-resistant laser leather transfer film according to claim 1, characterized in that: The thicknesses of the release layer, wear-resistant layer, molded color layer, plating layer and transfer adhesive layer are 1-2μm, 1-3μm, 1-2μm, 50-200nm and 1-5μm respectively. The molded color layer is obtained by molding after drying the color layer coating with a molding machine, wherein the color layer coating is composed of high-hydroxy acrylic resin, isocyanate curing agent, epoxy curing agent, color powder, dispersant and solvent in a mass ratio of 100:3-5:0.5-1:2-5:0.5-2:150-200.
7. The high-strength and wear-resistant laser leather transfer film according to claim 1, characterized in that: The transfer adhesive layer is formed by coating a transfer adhesive composed of a styrene thermoplastic elastomer, an epoxy resin, a thiol curing agent, and a solvent in a mass ratio of 100:15:5-8:150-200 and drying.
8. The high-strength and wear-resistant laser leather transfer film according to claim 1, characterized in that: The preparation method of the high-strength wear-resistant laser leather transfer film comprises the following steps: (1) firstly coating a UV release agent on the surface of the base film and irradiating the base film with UV light to form a release layer; (2) then applying a heated and melted wear-resistant coating on the surface of the release layer and drying it to form a wear-resistant layer; (3) coating a color layer coating on the surface of the wear-resistant layer, drying it to form a color layer, and then using a molding machine to mold the color layer to form a molded color layer, and then vacuum plating the surface to form an aluminum plating layer; (4) The coating surface is coated with transfer glue, which is dried to form a transfer glue layer, and then aged at 45° C. for 48 h. After cooling, a high-strength and wear-resistant laser leather transfer film is obtained.
Citation Information
Patent Citations
High-brightness and high-wear-resistance laser leather transfer film and preparation method thereof
CN114290846A