Photolysis glue for UTG glass and preparation method of photolysis glue

By using UV photosensitive expansion water-soluble bonding glue on UTG glass, combined with end hydroxyl polybutadiene polyurethane UV resin and end carboxy UV resin, the difficulties and environmental protection problems of traditional adhesives in fine cutting and processing of UTG glass are solved. It achieves the effect of having water resistance and cutting fluid resistance at room temperature, and quickly separating glass at high temperature.

CN118909587APending Publication Date: 2024-11-08GUANGZHOU YISHENG INVESTMENT PARTNERSHIP (LLP)
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411149952.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Traditional adhesives are difficult to remove in fine cutting of UTG glass. Strong acids or strong alkaline release agents are often required, which leads to glass corrosion and environmental protection problems, and it is difficult to have water resistance and cutting fluid resistance at room temperature.

Method used

Using 254-365nm wavelength UV photosensitive expansion water-soluble bonding adhesive, the film is formed through a 395nm LED light source, combined with end hydroxyl polybutadiene polyurethane UV resin and end carboxy UV resin to form a high-adhesive adhesive, and in UV light Under irradiation and high-temperature boiling, the glue bubbles and absorbs water and expands, and the glass is easily separated.

Benefits of technology

It realizes adhesives with excellent water resistance and cutting fluid resistance at room temperature, avoiding the use of strong acid and strong alkali release agents, which are safe and environmentally friendly, and quickly separate glass at high temperatures, improving processing efficiency and environmental protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005003362130000151
    Figure BDA0005003362130000151
  • Figure BDA0005003362130000161
    Figure BDA0005003362130000161
Patent Text Reader

Abstract

The invention provides a photolysis glue for UTG glass and a preparation method thereof, and relates to the technical field of photolysis glue preparation, and the photolysis glue comprises the following components by mass: 30-45 parts of hydroxyl-terminated polybutadiene polyurethane UV resin, 20-45 parts of carboxyl-terminated UV resin, 10-20 parts of a UV reactive diluent, 0.5-1 part of a photoinitiator, 8-16 parts of hydroxyl cyclohexane benzophenone, 0.5-2 parts of an antifoaming agent, 0.01-0.5 part of a polymerization inhibitor, 0.5-2 parts of a leveling agent, and 1-3 parts of an adherence promoter. The prepared photolysis glue for the UTG glass has excellent water resistance and cutting fluid resistance in a normal-temperature (45 DEG C or below) environment, so that an excellent protection effect on the whole CNC can be achieved, and the purpose of separating the glass is achieved by avoiding using a strong-acid and strong-alkali type release agent to remove the adhesive. In addition, the prepared photolysis glue for the UTG glass can separate the glass only by illumination and heating with water to 70-100 DEG C, and is safe, effective and environment-friendly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of photosolvent preparation, and in particular to a photosolvent for UTG glass and a preparation method thereof. Background Art

[0002] With the mass production and commercial use of ultra-thin flexible glass UTG (Ultra Thin Glass) cover plates for folding screens, UTG glass is increasingly used in mobile phones. However, because UTG glass is too thin and easy to break, it cannot be processed in a single piece. When doing fine cutting, in order to increase the yield, adhesives are often used to bond about 10 layers of glass together to increase the thickness of the glass, making it less easy to break before further fine cutting. Traditional adhesives, in order to be able to stick to UTG glass and withstand cutting fluid processing, often increase the acid, alkali and water resistance of the protective oil. After processing, it is extremely difficult to remove. Strong acid or strong alkaline deinking agents are often required for removal, and heating is required. Because UTG glass is too thin, it is often corroded by acids and alkalis when removing the adhesive, resulting in new defects. And the waste liquid after removal is not easy to handle.

[0003] In order to solve the above problems, it is urgent to develop a high-performance adhesive that can have excellent water resistance and cutting fluid resistance in a normal temperature (below 45°C) environment, so as to achieve the purpose of completing the protection effect of the entire CNC, and can remove the adhesive and separate the glass without strong acid and alkali release agents. There are also adhesives that can separate the glass under light, or have very strong hydrophilicity at higher temperatures (70°C to 100°C), and can quickly absorb water and swell to separate the glass within a few minutes. Nowadays, with the general improvement of social environmental awareness, the development of cleaner coatings has become an inevitable trend. Therefore, the development of an adhesive that is less harmful to the human body, can meet the cutting fluid processing environment, and does not require acid and alkali release agents, only UV debonding + hot water separation has great application prospects. Summary of the invention

[0004] In order to solve the above problems, the present invention aims to provide a 254-365nm wavelength UV light-sensitive swelling water-soluble adhesive and a preparation method thereof, wherein the adhesive is formed by a low-energy 395nm LED light source, and the glass has excellent adhesion after the adhesive is formed into a film. After curing, it can withstand cutting fluid at room temperature to complete the entire CNC process. The adhesive is first photolyzed with a 254-365nm wavelength UV to foam the glue, and then boiled in high-temperature boiling water to quickly absorb water and expand, thereby separating the UTG glass.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] The present invention provides a photosolvent for UTG glass, which comprises the following components in parts by mass:

[0007] 30-45 parts of terminal hydroxyl polybutadiene polyurethane type UV resin, 20-45 parts of terminal carboxyl UV resin, 10-20 parts of UV active diluent, 0.5-1 parts of photoinitiator, 8-16 parts of hydroxycyclohexane phenone, 0.5-2 parts of defoaming agent, 0.01-0.5 parts of inhibitor, 0.5-2 parts of leveling agent, and 1-3 parts of adhesion agent.

[0008] Further, based on the above technical solution, the carboxyl-terminated UV resin includes one or more of LUXYDIR ZHU-1998 or WS2100;

[0009] And / or, the mass ratio of the terminal hydroxyl polybutadiene polyurethane type UV resin to the terminal carboxyl UV resin is (1-2):(2-1), preferably 1:1.5.

[0010] Further, based on the above technical solution, the UV active diluent includes one or more of ACMO, IBOA or THFA.

[0011] Further, based on the above technical solution, the photoinitiator includes one or more of diphenyl-(2,4,6-trimethylbenzoyl)phosphine oxide, 2-phenylbenzyl-2-dimethylamine-1-(4-morpholinobenzylphenyl)butanone or 2-isopropylthioxanthone.

[0012] Further, based on the above technical solution, the defoaming agent is an organosilicon defoaming agent;

[0013] The organosilicon defoaming agent includes one or more of tego-900 or tego-810.

[0014] Further, based on the above technical solution, the inhibitor includes one or more of p-hydroxyanisole or tris(N-nitroso-N-phenylhydroxylamine)aluminum salt.

[0015] Further, based on the above technical solution, the leveling agent is a water-oil universal silicone leveling agent;

[0016] The water-oil universal silicone leveling agent includes one or more of BYK333 and TEGO Glide 410.

[0017] Further, based on the above technical solution, the adhesive agent is an epoxy silane coupling agent;

[0018] The epoxy silane coupling agent includes one or more of A-187, KBM-403 or Z-6040.

[0019] The present invention also provides a method for preparing the above-mentioned photosolvent for UTG glass, comprising the following steps:

[0020] Put terminal hydroxyl polybutadiene polyurethane type UV resin, terminal carboxyl UV resin, UV active diluent, photoinitiator, hydroxycyclohexane phenone, defoamer, polymerization inhibitor, leveling agent and adhesion agent into a blender, stir and filter to obtain photosol for UTG glass.

[0021] Furthermore, based on the above technical solution, the stirring rate is 100-150 r / min, the temperature is 24-35° C., and the stirring time is 50-70 min.

[0022] The present invention provides a photosolvent for UTG glass and a preparation method thereof, and the beneficial effects are as follows:

[0023] 1. The present invention adopts terminal hydroxyl polybutadiene polyurethane type UV resin as one of the main components of the photosol for UTG glass. Since the molecular skeleton of terminal hydroxyl polybutadiene is mainly composed of carbon-carbon single bonds and has a hydroxyl group at the end, the terminal hydroxyl polybutadiene does not contain ether bonds or ester bonds. Therefore, the terminal hydroxyl polybutadiene polyurethane type UV resin has good hydrolysis stability. When the prepared photosol is cured by using LED, it will produce good viscosity and good adhesion to glass. In addition, the terminal hydroxyl polybutadiene polyurethane type UV resin also has excellent acid resistance, mechanical properties and high elongation.

[0024] 2. The present invention adopts carboxyl-terminated UV resin as one of the main components of the photosolvent for UTG glass because the carboxyl-terminated UV resin has the characteristics of high TG, high hardness and high functional group. This is because the highly functional carboxyl-terminated UV resin can participate in the cross-linking reaction to form a highly cross-linked three-dimensional network structure, increase the molecular weight and cross-linking density of the resin, and further improve the viscosity and acid resistance of the photosolvent.

[0025] 3. The present invention limits the mass ratio of the hydroxyl-terminated polybutadiene polyurethane type UV resin to the carboxyl-terminated UV resin to (1-2): (2-1) because when the high-hardness carboxyl-terminated UV resin and the high-elongation hydroxyl-terminated polybutadiene polyurethane type UV resin interact with each other, due to the difference in their physical properties, a slight stress difference may be generated during the curing process, resulting in the formation of tiny bubbles or gaps between the glue film layer and the glass substrate, which looks like bubbles. In this way, it is easier for water to enter the glue layer through the gaps of the bubbles during boiling, thereby achieving the separation of the photodissolved glue from the glass, and the carboxyl group, as a hydrophilic group, has strong water absorption. During the boiling process, the carboxyl group will absorb a large amount of water, causing the volume of the photodissolved glue to expand, further aggravating the separation from the glass. At the same time, water enters the glue layer through the gaps of the bubbles, weakening the adhesion between the glue layer and the glass, and finally achieving easy separation of the photodissolved glue from the glass.

[0026] 4. The present invention solves the problem of the corrosion of the UTG glass substrate by common deinking agents, avoids the blueing of UTG glass, and only uses energy of 20000-30000 J / cm 2 The adhesive is irradiated with UV light from a mercury lamp until bubbles appear, and then heated with water to 70℃~80℃ to separate the glass. This is effective, safe and environmentally friendly.

[0027] 5. The photodissolved adhesive provided by the present invention utilizes a 395nm LED light source for low-energy film formation. After the photodissolved adhesive is formed, it has excellent adhesion to glass at room temperature (below 45°C), and has excellent water resistance and glass cutting fluid performance, thereby achieving the purpose of protecting the entire CNC.

[0028] 6. After CNC processing, the photolytic glue provided by the present invention absorbs 20000-30000 J / cm 2 After being exposed to 254-365nm UV light from a high-pressure mercury lamp, it undergoes cracking and bubbling. At higher temperatures (70℃~100℃), it has very strong hydrophilicity and can quickly absorb water and swell within a dozen minutes to separate the glass.

[0029] 7. The preparation method of the photolytic gel provided by the present invention is convenient, safe and more efficient during production and use. DETAILED DESCRIPTION

[0030] In order to make the purpose, technical scheme and advantages of the present invention clearer, the technical scheme in the embodiment of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention. The process parameters of the following embodiments that do not specify specific conditions are usually based on conventional conditions.

[0031] The endpoints and any values ​​of the ranges disclosed in the present invention are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be regarded as specifically disclosed in the present invention.

[0032] According to a first aspect of the present invention, a photosolvent for UTG glass is provided, comprising the following components in parts by mass:

[0033] 30-45 parts of terminal hydroxyl polybutadiene polyurethane type UV resin, 20-45 parts of terminal carboxyl UV resin, 10-20 parts of UV active diluent, 0.5-1 parts of photoinitiator, 8-16 parts of hydroxycyclohexane phenone (184), 0.5-2 parts of defoaming agent, 0.01-0.5 parts of inhibitor, 0.5-2 parts of leveling agent, and 1-3 parts of adhesion agent.

[0034] Specifically, the UTG glass photosolvent prepared by the present invention can have excellent water resistance and cutting fluid resistance at room temperature (below 45°C), thereby having excellent protection effect on the entire CNC, and avoiding the use of strong acid and strong alkali type release agents to remove adhesives, thereby achieving the purpose of separating glass. Moreover, the UTG glass photosolvent prepared by the present invention only needs to be separated by light + heating with water to 70°C to 100°C, which is safe, effective and environmentally friendly.

[0035] Specifically, the present invention adopts terminal hydroxyl polybutadiene polyurethane type UV resin as one of the main components of the photosol for UTG glass. Since the molecular skeleton of the terminal hydroxyl polybutadiene is mainly composed of carbon-carbon single bonds and has a hydroxyl group at the end, the terminal hydroxyl polybutadiene does not contain ether bonds or ester bonds. Therefore, the terminal hydroxyl polybutadiene polyurethane type UV resin has good hydrolysis stability. When the prepared photosol is cured using LED, it will produce good viscosity and good adhesion to glass. The terminal hydroxyl polybutadiene polyurethane type UV resin also has excellent acid resistance, mechanical properties and high elongation.

[0036] As an optional embodiment of the present invention, the carboxyl-terminated UV resin includes one or more of LUXYDIR ZHU-1998 or WS2100;

[0037] And / or, the mass ratio of the hydroxyl-terminated polybutadiene polyurethane type UV resin to the carboxyl-terminated UV resin is (1-2):(2-1) (such as 1:2, 1:1.5, 1:1, 2:1, 1.5:1, etc.), preferably 1:1.5.

[0038] Specifically, the carboxyl-terminated UV resin used in the present invention has the characteristics of high TG, high hardness, and high functional groups. This is because the highly functional carboxyl-terminated UV resin can participate in the cross-linking reaction to form a highly cross-linked three-dimensional network structure, increase the molecular weight and cross-linking density of the resin, and further improve the viscosity and acid resistance of the photolytic gel;

[0039] Furthermore, the present invention limits the mass ratio of the terminal hydroxyl polybutadiene polyurethane type UV resin and the terminal carboxyl UV resin to (1-2): (2-1) because when the high-hardness terminal carboxyl UV resin and the high-elongation terminal hydroxyl polybutadiene polyurethane type UV resin interact with each other, due to the difference in their physical properties, a slight stress difference may be generated during the curing process, resulting in the formation of tiny bubbles or gaps between the glue film layer and the glass substrate, which looks like bubbles. In this way, it is easier for water to enter the glue layer through the gaps of the bubbles during boiling, thereby achieving the separation of the photodissolved glue and the glass, and the carboxyl group, as a hydrophilic group, has strong water absorption. During the boiling process, the carboxyl group will absorb a large amount of water, causing the volume of the photodissolved glue to expand, further exacerbating the separation from the glass. At the same time, water enters the glue layer through the gaps of the bubbles, weakening the adhesion between the glue layer and the glass, and finally achieving easy separation of the photodissolved glue and the glass.

[0040] As an optional embodiment of the present invention, the UV active diluent includes one or more of ACMO, IBOA or THFA.

[0041] Specifically, in the present invention, the UV active diluent plays the role of dissolving the photoinitiator and hydroxycyclohexane phenone, so that the present invention does not need to add additional solvent and can mix all the raw materials evenly; and the UV active diluent also plays the role of adjusting viscosity and increasing curing speed.

[0042] It can undergo polymerization reaction with the active intermediates produced by the photoinitiator and become part of the cured film. Due to this chemical structure characteristic, UV reactive diluents can effectively dissolve solid components such as photoinitiators and hydroxycyclohexane phenone, so that all raw materials can be mixed evenly without the need to add additional volatile organic solvents to form a stable UV curing system; secondly, UV reactive diluents play an important role in adjusting the viscosity of the system, and UV reactive diluents can also significantly increase the curing speed. Because they contain polymerizable functional groups, they can quickly participate in the polymerization reaction under the action of photoinitiators to form a cross-linked network structure and accelerate the curing process. This fast curing characteristic makes UV curing technology have the advantages of high efficiency, energy saving and environmental protection.

[0043] As an optional embodiment of the present invention, the photoinitiator includes one or more of diphenyl-(2,4,6-trimethylbenzoyl)phosphine oxide (TPO), 2-phenylbenzyl-2-dimethylamine-1-(4-morpholinobenzylphenyl)butanone or 2-isopropylthioxanthone.

[0044] Specifically, the main function of the photoinitiator is to absorb 395nm light during LED curing of the photosol, decompose to produce active intermediates such as free radicals or cations, and these active intermediates further initiate the polymerization reaction of the carboxyl-terminated UV resin and the hydroxyl-terminated polybutadiene polyurethane type UV resin, thereby achieving rapid curing of the photosol.

[0045] Photoinitiators can absorb 395nm light when the photosol is LED cured, and then produce compounds with active intermediates such as free radicals and cations; the generated active intermediates such as free radicals or cations are highly reactive and can further initiate the polymerization reaction of carboxyl-terminated UV resins and hydroxyl-terminated polybutadiene polyurethane-type UV resins. Under the action of active intermediates, carboxyl UV resins and hydroxyl-terminated polybutadiene polyurethane-type UV resins gradually cross-link and cure into a polymer network structure through the formation and growth of chemical bonds, thereby achieving rapid curing of the photosol; and the application of photoinitiators significantly improves the curing efficiency and performance of the photosol. At the same time, since no or very little solvent is required during the photocuring process, the emission of volatile organic compounds is also reduced, which is more environmentally friendly.

[0046] Specifically, hydroxycyclohexane phenone also plays a role in accelerating curing. During the UV curing process, it can quickly absorb light energy under the irradiation of ultraviolet light and convert it into chemical energy, thereby initiating rapid curing of the photodisintegrator.

[0047] As an optional embodiment of the present invention, the defoaming agent is an organosilicon defoaming agent;

[0048] The organosilicon defoaming agent includes one or more of tego-900 or tego-810.

[0049] Specifically, the main function of the defoamer is to eliminate the foam generated during the production and construction of the glue. After the defoamer is added, it is not easy to foam when preparing the glue, but a small amount of foam will also be generated when the rotation speed is fast. In order to suppress the foam, an additional 0.2-0.5 parts of silicone defoamer can be added.

[0050] As an optional embodiment of the present invention, the inhibitor includes one or more of p-hydroxyanisole or tris(N-nitroso-N-phenylhydroxylamine)aluminum salt.

[0051] Specifically, photoresist usually contains chemicals that can undergo polymerization reactions in response to light. However, in the absence of light, if the storage or transportation conditions are improper, these chemicals may also undergo slow polymerization reactions, causing the photoresist to be partially or completely solidified before use, thereby losing its application value. Inhibitors improve the stability of photoresist by inhibiting or delaying the progress of these chemical reactions. Inhibitors can bind to the active sites that initiate polymerization reactions to form stable compounds, thereby preventing the initiation of polymerization reactions or slowing down their progress. In this way, even during long-term storage or transportation, the photoresist can maintain its original fluidity and reactivity, ensuring that it can be used normally when needed.

[0052] As a preferred embodiment of the present invention, the leveling agent is a water-oil universal silicone leveling agent;

[0053] The water-oil universal silicone leveling agent includes one or more of BYK333 and TEGO Glide 410.

[0054] Specifically, the main function of the leveling agent is to make the photodissolved glue have higher spreadability during use. The present invention is further defined as a water-oil universal silicone leveling agent, which not only has a wider range of applications, but also for water-based glue systems, the use of this leveling agent helps to reduce the emission of volatile organic compounds (VOCs).

[0055] As a preferred embodiment of the present invention, the adhesive agent is an epoxy silane coupling agent;

[0056] The epoxy silane coupling agent includes one or more of A-187, KBM-403 or Z-6040.

[0057] Specifically, the epoxy silane coupling agent will hydrolyze to generate oligomers containing silanol (Si-OH), which will further undergo condensation reactions to form a siloxane network. At the same time, the silanol can also react with the hydroxyl provided by the terminal hydroxyl polybutadiene to generate silicon-oxygen bonds (Si-OC) and carbon-oxygen bonds (COC), effectively improving the adhesion between the photoresist and the glass.

[0058] Epoxysilane coupling agents contain hydrolyzable epoxy groups and silane groups in their molecules. When these coupling agents are exposed to water or moisture, the silane groups undergo hydrolysis to generate silanol groups (Si-OH). The generated silanol groups (Si-OH) are highly reactive and can further undergo condensation reactions (also known as dehydration condensation) to form siloxane bonds (Si-O-Si). This process causes the oligomers to gradually crosslink into a three-dimensional network structure, namely the siloxane network. This network structure not only enhances the cohesive strength of the photosol, but also provides a stable skeleton for its bonding with the glass, increases the cohesive strength and toughness of the photosol, enables it to better adapt to and fill the tiny bumps on the glass surface, and forms a mechanical locking effect. At the same time, the silanol groups (Si-OH) can also react with the hydroxyl groups in the hydroxy-terminated polybutadiene. This reaction is usually carried out through the initial formation of hydrogen bonds and subsequent dehydration condensation to generate silicon oxygen bonds (Si-OC) and carbon oxygen bonds (COC). The formation of these chemical bonds firmly connects the organic components in the photoresist to the inorganic substrate (such as silanol groups or silanol groups on glass), thereby significantly improving the adhesion between the two.

[0059] According to a second aspect of the present invention, there is provided a method for preparing the above-mentioned photosolvent for UTG glass, comprising the following steps:

[0060] Put terminal hydroxyl polybutadiene polyurethane type UV resin, terminal carboxyl UV resin, UV active diluent, photoinitiator, hydroxycyclohexane phenone, defoamer, polymerization inhibitor, leveling agent and adhesion agent into a blender, stir and filter to obtain photosol for UTG glass.

[0061] Specifically, the present invention adds all raw materials to the stirring device at one time for mixing, avoids the complexity of adding raw materials in steps, and makes the whole operation process intuitive and easy to control. This not only reduces the requirements for operator skills, but also reduces the possibility of operating errors; when all raw materials are mixed in a closed or well-ventilated stirring device, the volatilization and leakage of harmful substances can also be effectively reduced, thereby reducing the harm to operators and the environment; in addition, one-time mixing also reduces the number of direct contact with raw materials, further reducing safety risks; due to the elimination of the time interval and waiting process of step-by-step mixing, this one-time mixing method significantly improves production efficiency. The stirring device usually has an efficient mixing capacity, which can mix the raw materials evenly in a short time, providing a good foundation for subsequent processing steps. This method of mixing all raw materials together can easily meet the needs of large-scale production and ensure that each batch of products has the same quality and performance. At the same time, due to its simple operation and high efficiency, this method also helps to reduce production costs and improve market competitiveness.

[0062] As a preferred embodiment of the present invention, the stirring rate is 100-150 r / min, the temperature is 24-35° C., and the stirring time is 50-70 min.

[0063] The present invention will be further described in detail below with reference to specific embodiments and comparative examples.

[0064] Example 1

[0065] 30 parts of hydroxy-terminated polybutadiene polyurethane type UV resin;

[0066] Carboxyl-terminated UV resin: 45 parts of LUXYDIR ZHU-1998;

[0067] UV active diluent: ACMO 14.95 parts;

[0068] Photoinitiator: 0.5 parts of diphenyl-(2,4,6-trimethylbenzoyl)phosphine oxide (TPO);

[0069] Hydroxycyclohexane phenone: 8 parts;

[0070] Defoaming agent: tego-9000.5 parts;

[0071] Inhibitor: p-hydroxyanisole 0.01 parts;

[0072] Leveling agent: BYK3332 parts;

[0073] Adhesive: A-1871.99 parts;

[0074] The above raw materials were placed in a stirrer, stirred at a temperature of 30° C. and a stirring rate of 100 r / min for 60 min, and filtered to obtain a photosol for UTG glass.

[0075] Example 2

[0076] 32 parts of hydroxy-terminated polybutadiene polyurethane type UV resin;

[0077] Carboxyl-terminated UV resin: WS2100 34 parts;

[0078] UV active diluent: IBOA 20 parts;

[0079] Photoinitiator: 0.8 parts of 2-phenylbenzyl-2-dimethylamine-1-(4-morpholinobenzylphenyl)butanone;

[0080] 10 parts of hydroxycyclohexane phenone;

[0081] Defoaming agent: 1 part of tego-8;

[0082] Inhibitor: 0.4 parts of tris(N-nitroso-N-phenylhydroxylamine)aluminum salt;

[0083] Leveling agent: TEGO Glide 4100.8 parts;

[0084] Adhesive agent: KBM-403 1 part;

[0085] The above raw materials were placed in a stirrer, stirred at a temperature of 35° C. and a stirring rate of 150 r / min for 50 min, and filtered to obtain a photosol for UTG glass.

[0086] Example 3

[0087] 40 parts of hydroxy-terminated polybutadiene polyurethane type UV resin;

[0088] Carboxyl-terminated UV resin: 26 parts of LUXYDIR ZHU-1998 and WS2100;

[0089] UV active diluent: THFA 14 parts;

[0090] Photoinitiator: 1 part of 2-isopropylthioxanthone;

[0091] 14 parts of hydroxycyclohexane phenone;

[0092] Defoaming agent: 1.8 parts of tego-900 and tego-810;

[0093] Inhibitor: 0.2 parts of p-hydroxyanisole;

[0094] Leveling agent: BYK3331.5 parts;

[0095] Adhesive agent: Z-6040 1.5 parts;

[0096] The above raw materials were placed in a mixer, stirred at a temperature of 24° C. and a stirring rate of 120 r / min for 70 min, and filtered to obtain a photosol for UTG glass.

[0097] Example 4

[0098] 45 parts of hydroxy-terminated polybutadiene polyurethane type UV resin;

[0099] Carboxyl-terminated UV resin: 22 parts of LUXYDIR ZHU-1998;

[0100] UV active diluent: IBOA 10 parts;

[0101] Photoinitiator: 1 part of diphenyl-(2,4,6-trimethylbenzoyl)phosphine oxide;

[0102] 16 parts of hydroxycyclohexane phenone;

[0103] Defoaming agent: 2 parts of tego-900;

[0104] Inhibitor: 0.5 parts of tris(N-nitroso-N-phenylhydroxylamine)aluminum salt;

[0105] Leveling agent: TEGO Glide 4100.5 parts;

[0106] Adhesive agent: KBM-4033 parts;

[0107] The above raw materials were placed in a stirrer, stirred at a temperature of 25° C. and a stirring rate of 100 r / min for 50-70 min, and filtered to obtain a photosol for UTG glass.

[0108] Comparative Example 1

[0109] 21.95 parts of hydroxy-terminated polybutadiene polyurethane type UV resin;

[0110] Carboxyl-terminated UV resin: 52 parts of LUXYDIR ZHU-1998;

[0111] UV active diluent: ACMO 15 parts;

[0112] Photoinitiator: 0.5 parts of diphenyl-(2,4,6-trimethylbenzoyl)phosphine oxide;

[0113] Hydroxycyclohexane phenone 9 parts;

[0114] Defoaming agent: tego-9000.5 parts;

[0115] Inhibitor: 0.05 parts of p-hydroxyanisole;

[0116] Leveling agent: BYK3331 parts;

[0117] Adhesive: A-1871 parts;

[0118] The above raw materials were placed in a stirrer, stirred at a temperature of 30° C. and a stirring rate of 100 r / min for 60 min, and filtered to obtain a photosol for UTG glass.

[0119] Comparative Example 2

[0120] 59 parts of hydroxy-terminated polybutadiene polyurethane type UV resin;

[0121] Carboxyl-terminated UV resin: 15 parts of LUXYDIR ZHU-1998;

[0122] UV active diluent: ACMO 10.95 parts;

[0123] Photoinitiator: 0.5 parts of diphenyl-(2,4,6-trimethylbenzoyl)phosphine oxide;

[0124] 10 parts of hydroxycyclohexane phenone;

[0125] Defoaming agent: tego-9000.5 parts;

[0126] Inhibitor: 0.05 parts of p-hydroxyanisole;

[0127] Leveling agent: BYK3332 parts;

[0128] Adhesive: A-1872 parts;

[0129] The above raw materials were placed in a stirrer, stirred at a temperature of 30° C. and a stirring rate of 100 r / min for 60 min, and filtered to obtain a photosol for UTG glass.

[0130] Comparative Example 3

[0131] 25 parts of hydroxy-terminated polybutadiene polyurethane type UV resin;

[0132] Carboxyl-terminated UV resin: 54 parts of LUXYDIR ZHU-1998;

[0133] UV active diluent: ACMO 9.45 parts;

[0134] Photoinitiator: 0.5 parts of diphenyl-(2,4,6-trimethylbenzoyl)phosphine oxide;

[0135] 7 parts of hydroxycyclohexane phenone;

[0136] Defoaming agent: tego-9000.5 parts;

[0137] Inhibitor: 0.05 parts of p-hydroxyanisole;

[0138] Leveling agent: BYK3331.5 parts;

[0139] Adhesive: A-1872 parts;

[0140] The above raw materials were placed in a stirrer, stirred at a temperature of 30° C. and a stirring rate of 100 r / min for 60 min, and filtered to obtain a photosol for UTG glass.

[0141] Comparative Example 4

[0142] 40 parts of hydroxy-terminated polybutadiene polyurethane type UV resin;

[0143] Carboxyl-terminated UV resin: 32.5 parts of LUXYDIR ZHU-1998;

[0144] UV active diluent: ACMO 10.95 parts;

[0145] Photoinitiator: 0.5 parts of diphenyl-(2,4,6-trimethylbenzoyl)phosphine oxide;

[0146] 14 parts of hydroxycyclohexane phenone;

[0147] Defoaming agent: tego-9000.5 parts;

[0148] Inhibitor: 0.05 parts of p-hydroxyanisole;

[0149] Leveling agent: BYK3331 parts;

[0150] Adhesive: A-1870.5 parts;

[0151] The above raw materials were placed in a stirrer, stirred at a temperature of 30° C. and a stirring rate of 100 r / min for 60 min, and filtered to obtain a photosol for UTG glass.

[0152] Performance Test:

[0153] The curing steps include:

[0154] (1) Clean the glass surface;

[0155] (2) Prepare the light source: the light source is UVLED;

[0156] (3) Gluing:

[0157] The photodissolved adhesive prepared in Examples 1-4 and Comparative Examples 1-4 is uniformly coated on the glass surface;

[0158] (4) Curing:

[0159] Setting parameters: curing energy is 300j / cm 2 , wavelength 254~365nm, time 10min;

[0160] Irradiation curing: Input the set parameters into the UVLED light source device and start the device. The UVLED light source emits ultraviolet light with a wavelength of 254 to 365nm, which is irradiated onto the glass surface coated with the photodissolved adhesive. Under the irradiation of ultraviolet light, the photodissolved adhesive will quickly undergo a curing reaction to form a solid structure.

[0161] The standard for the grid attachment is ASTM D3359;

[0162] Acid resistance: Place the UTG glass with photoresist glue attached in 10% HF and soak it at 30℃ for 20 minutes to observe whether the photoresist glue dissolves and falls off.

[0163] Degumming process:

[0164] 1. Place the UTG glass with photodissolved adhesive under the energy of 20000~30000J / cm 2 Irradiate with UV light under a mercury lamp for 1-2 hours and observe whether the photodissolved glue bubbles;

[0165] 2. Boil the UTG glass with bubbling photodissolved glue in hot water at 90°C, calculate the time when the photodissolved glue falls off, and observe whether there is any residue on the UTG glass.

[0166] Table 1 Components and their corresponding mass percentages in Examples 1-4 and Comparative Examples 1-4

[0167]

[0168]

[0169] As shown in Table 1, compared with Example 1, since the contents of the terminal hydroxyl polybutadiene polyurethane type UV resin and the terminal carboxyl UV resin in Comparative Example 1 are both beyond the range defined in the present invention, and the content of the terminal carboxyl UV resin is significantly higher than that of the terminal hydroxyl polybutadiene polyurethane type UV resin, and the content of high functional groups is too much, the viscosity of the photosol is significantly increased when the two interact with each other, so the amount of foaming is less during the curing process, so the degumming time is increased, and the high content of the terminal hydroxyl polybutadiene polyurethane type UV resin further affects the crosslinking density when the two resins interact with each other, thereby reducing the acid resistance of the photosol.

[0170] As shown in Table 1, compared with Example 1, in Comparative Example 2, since the contents of the terminal hydroxyl polybutadiene polyurethane type UV resin and the terminal carboxyl UV resin in Comparative Example 2 are both beyond the range defined in the present invention, and the content of the terminal hydroxyl polybutadiene polyurethane type UV resin is significantly higher than that of the terminal carboxyl UV resin, a high content of the terminal hydroxyl polybutadiene polyurethane type UV resin will significantly increase the viscosity of the photosol, resulting in residual photosol on the glass after the degumming operation.

[0171] As shown in Table 1, compared with Example 1, in Comparative Example 3, not only the contents of the hydroxyl-terminated polybutadiene polyurethane type UV resin and the carboxyl-terminated UV resin in Comparative Example 3 are beyond the scope defined in the present invention, but the contents of the UV active diluent and hydroxycyclohexane phenone are also outside the scope defined in the present invention, the viscosity regulating effect of the UV active diluent on the photosol is weakened, the carboxyl-terminated UV resin causes the viscosity of the photosol to increase, and even causes no bubbling during the curing process, so after the degumming operation, there is still residual photosol on the glass.

[0172] As shown in Table 1, compared with Example 1, since the adhesive in Comparative Example 4 is not within the scope defined by the present invention, the content of the adhesive is reduced, resulting in reduced adhesion between the photolytic adhesive and the glass. When the acid resistance test is performed, dissolution and shedding easily occur.

[0173] In summary, the present invention uses a high-hardness carboxyl-terminated UV resin and a high-elongation hydroxyl-terminated polybutadiene polyurethane UV resin to prepare UTG photodissolver, and strictly limits the ratio of the two. Therefore, when the two interact with each other, due to the difference in physical properties, a small stress difference may be generated during the curing process, resulting in the formation of tiny bubbles or gaps between the glue film layer and the glass substrate, which looks like bubbles. In this way, it is easier for water to enter the glue layer along the gaps of the bubbles during boiling, thereby achieving the separation of the photodissolver from the glass, and the carboxyl group, as a hydrophilic group, has strong water absorption. During the boiling process, the carboxyl group will absorb a large amount of water, causing the volume of the photodissolver to expand, further exacerbating the separation from the glass. At the same time, water enters the glue layer through the gaps of the bubbles, weakening the adhesion between the glue layer and the glass, and finally achieving easy separation of the photodissolver from the glass.

[0174] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A photodissolver for UTG glass, characterized in that: Calculated by mass, it includes the following components: 30-45 parts of terminal hydroxyl polybutadiene polyurethane type UV resin, 20-45 parts of terminal carboxyl UV resin, 10-20 parts of UV active diluent, 0.5-1 parts of photoinitiator, 8-16 parts of hydroxycyclohexane phenone, 0.5-2 parts of defoaming agent, 0.01-0.5 parts of inhibitor, 0.5-2 parts of leveling agent, and 1-3 parts of adhesion agent.

2. The photosol for UTG glass according to claim 1, characterized in that: The carboxyl-terminated UV resin includes one or more of LUXYDIR ZHU-1998 or WS2100; And / or, the mass ratio of the terminal hydroxyl polybutadiene polyurethane type UV resin to the terminal carboxyl UV resin is (1-2):(2-1), preferably 1:1.

5.

3. The photosol for UTG glass according to claim 1, characterized in that: The UV active diluent includes one or more of ACMO, IBOA or THFA.

4. The photosol for UTG glass according to claim 1, characterized in that: The photoinitiator includes one or more of diphenyl-(2,4,6-trimethylbenzoyl)phosphine oxide, 2-phenylbenzyl-2-dimethylamine-1-(4-morpholinobenzylphenyl)butanone or 2-isopropylthioxanthone.

5. The photosol for UTG glass according to claim 1, characterized in that: The defoamer is an organosilicon defoamer; The organosilicon defoaming agent includes one or more of tego-900 or tego-810.

6. The photosol for UTG glass according to claim 1, characterized in that: The inhibitor includes one or more of p-hydroxyanisole and tris(N-nitroso-N-phenylhydroxylamine)aluminum salt.

7. The photosol for UTG glass according to claim 1, characterized in that: The leveling agent is a water-oil universal silicone leveling agent; The water-oil universal silicone leveling agent includes one or more of BYK333 and TEGO Glide 410.

8. The photosol for UTG glass according to claim 7, characterized in that: The adhesive is an epoxy silane coupling agent; The epoxy silane coupling agent includes one or more of A-187, KBM-403 or Z-6040.

9. A method for preparing a photosol for UTG glass according to any one of claims 1 to 8, characterized in that: The steps include: Put terminal hydroxyl polybutadiene polyurethane type UV resin, terminal carboxyl UV resin, UV active diluent, photoinitiator, hydroxycyclohexane phenone, defoamer, polymerization inhibitor, leveling agent and adhesion agent into a blender, stir and filter to obtain photosol for UTG glass.

10. The method for preparing photosol for UTG glass according to claim 9, characterized in that: The stirring rate is 100-150 r / min, the temperature is 24-35° C., and the stirring time is 50-70 min.