Two-component flocking interface adhesive as well as preparation method and flocking method thereof

Through the preparation of two-component flocking interface glue, the polymerization reaction of hydroxyacrylic emulsion and aqueous isocyanate is used, combined with wetting agents and cationic dispersants, the surface bonding problem of different substrates is solved, the adhesion and water resistance are improved, and the adhesion and water resistance are extended. The film formation opening time has been improved, and the decoration effect and construction convenience are improved.

CN119019971APending Publication Date: 2024-11-26HANGZHOU LINAN PRACTICAL DECORATION MATERIALS CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410926000.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The prior art is difficult to effectively bond velvet on the surfaces of different substrates, resulting in glue removal, glue leakage and bubble phenomena, affecting the decorative effect, and the film formation opening time of the interface glue is not suitable, limiting the construction time.

Method used

Two-component flocking interface glue is used to prepare glue by mixing hydroxyacrylic emulsion with aqueous isocyanate, adding wetting agent, cationic dispersant and defoaming agent to control surface tension and pigment dispersion, extend film formation opening time, and improve adhesion and water resistance.

Benefits of technology

It realizes efficient bonding of velvets on the surfaces of different substrates, enhances water resistance and aging resistance, extends the film formation opening time, and improves the decorative effect and construction convenience.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a two-component flocking interface adhesive. The two-component flocking interface adhesive is composed of a first component glue and a second component curing agent, the first component glue is prepared from the following components in parts by weight: 30 to 60 parts of hydroxyl acrylic emulsion, 36.5 to 70 parts of hydroxyethyl cellulose aqueous solution, 0.1 to 0.5 part of wetting agent, 0.1 to 0.5 part of defoaming agent and 0.3 to 0.5 part of cationic dispersant; the second component curing agent comprises the following components in parts by weight: 6-12 parts of water-based isocyanate and 1-3 parts of a diethylene glycol monobutyl ether solvent; the solid content of the hydroxy acrylic emulsion is 42-48%, and the solid content of the water-based isocyanate is 80-100%; according to the preparation of the two-component flocking interface adhesive, hydroxyl acrylic emulsion and waterborne isocyanate are mixed, hydroxyl and an NCO group are subjected to a polymerization reaction to prepare the adhesive, and the hydroxyl acrylic emulsion has good film-forming performance, weather resistance, acid resistance and alkali resistance and can improve the crosslinking density and adhesive force of a paint film; the prepared glue can form a glue film with excellent water resistance and super-strong adhesive force, then the wetting agent is used for controlling the surface tension of the glue film and increasing the adhesive force to a base material, the cationic dispersing agent is used for better dispersing pigment, an anode electric field surface is provided, the opening time of double-component flocking interface glue film forming is prolonged, and the double-component flocking interface glue film forming effect is improved. The water resistance and the adhesive force are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of flocking adhesive, in particular to a two-component flocking interface adhesive and a preparation method thereof and a flocking method. Background Art

[0002] Flocking is a technology that fixes short fibers vertically to the surface of the substrate. The short fibers are usually nylon, polyester or other synthetic materials. The flocking surface has the characteristics of softness, smoothness and wear resistance.

[0003] Large-area building interior walls, plastics, metal plates and other substrate surfaces require a product with a gentle touch, rich colors, super strong stain resistance, weather resistance, and antioxidant ability, and the flocking decoration effect is very beautiful and high-end. However, general composite glue is not suitable for bonding different substrate surfaces. The film-forming open time of the glue is very critical. If the open time is too long, the flocking hair will easily fall and not be perpendicular to the facade. If the open time is too short, the film cannot be constructed because it forms too quickly, or the construction time is limited. According to the inconsistency of the surface tension of different substrates, the interface glue should effectively wet the surface, otherwise it will cause glue running, glue leakage, bubbles and other phenomena, affecting the decorative effect.

[0004] Therefore, a new type of flocking interface glue is needed to bond the fluff and different substrates to improve the anti-aging and decorative effects of different substrates. The interface glue is one of the core materials for facade flocking. Its main function is to bond the surfaces of different substrates with the fluff and provide a rich and colorful base color. At the same time, the interface glue is environmentally friendly, non-toxic, zero VOC, mildew-proof, and has the advantages of strong adhesion, aging resistance, and water resistance. Summary of the invention

[0005] The object of the present invention is to provide a two-component flocking interface adhesive and a preparation method thereof, so as to solve the problems raised in the above background technology.

[0006] To achieve the above object, the present invention provides the following technical solutions: a two-component flocking interface adhesive, the two-component flocking interface adhesive is composed of a first component of glue and a second component of curing agent; The first component of glue comprises the following components and weight parts: 30-60 parts of hydroxy acrylic emulsion, 36.5-70 parts of hydroxyethyl cellulose aqueous solution, 0.1-0.5 parts of wetting agent, 0.1-0.5 parts of defoaming agent, and 0.3-0.5 parts of cationic dispersant; The second component curing agent includes the following ingredients and weight parts: 6-12 parts of water-based isocyanate and 1-3 parts of diethylene glycol butyl ether solvent; The solid content of the hydroxy acrylic emulsion is 42-48%, and the solid content of the water-based isocyanate is 80-100%.

[0007] Preferably, the raw materials of the first component glue further include 1 to 2 parts by weight of pigment; The hydroxylated acrylic emulsion includes a hydroxylated acrylic emulsion with the brand name of Double Bond Chemical DB3650; The wetting agent is a cationic wetting agent or a nonionic wetting agent; The defoamer is an organosilicon defoamer; The cationic dispersant includes a cationic dispersant with the brand name of TEGO 690; The water-based isocyanate includes a water-based isocyanate with the brand name of Double Bond Chemical DB82547; The diethylene glycol butyl ether solvent includes diethylene glycol butyl ether solvents with the brands of DOW DB and DOW DOWANOL DBA.

[0008] Preferably, the weight ratio of the hydroxylated acrylic emulsion contained in the first component of the glue to the aqueous isocyanate contained in the second component of the curing agent is 5:1.

[0009] Preferably, the hydroxyethyl cellulose aqueous solution comprises the following components and weight parts: 1-3 parts of hydroxyethyl cellulose, 1-3 parts of ammonia neutralizer, and 96-98 parts of water; The ammonia neutralizer includes Henkel OP-10 and Dow AMP-95. The hydroxyethyl cellulose and the ammonia neutralizer are mixed with water to obtain a hydroxyethyl cellulose aqueous solution.

[0010] Preferably, the pH value of the hydroxyethyl cellulose aqueous solution is 8-9, the reaction temperature for preparing the hydroxyethyl cellulose aqueous solution is 10-40° C., and the reaction time is 12-36 hours.

[0011] Preferably, the preparation method of the two-component flocking interface adhesive comprises the following steps: (a), mixing a hydroxy acrylic acid emulsion with a hydroxyethyl cellulose aqueous solution to obtain a mixture A; (b), mixing the wetting agent, the cationic dispersant and the defoaming agent with the mixture A to obtain a mixture B; (c) mixing the mixture B with the pigment to obtain a first component of glue; (d) mixing water-based isocyanate with diethylene glycol butyl ether solvent to obtain a second component curing agent; (e) Mix the first component glue and the second component curing agent to obtain a two-component flocking interface glue.

[0012] Preferably, the mixing speed for preparing the two-component flocking interface adhesive is 300~1500r / min, the reaction temperature is 10~40°C, in the step a, the reaction time is 5~10min, in the step b, the reaction time is 5~10min, in the step c, the reaction time is 20~30min, in the step d, the reaction time is 15~30min, and in the step e, the reaction time is 5~10min.

[0013] Preferably, the room temperature viscosity of the two-component flocking interface adhesive is 200-300 KU.

[0014] Preferably, the facade flocking method comprises the following steps: S1: pre-treating the substrate surface; S2: Apply the two-component flocking interface adhesive to the surface of the substrate; S3: electrostatic flocking is performed on the surface of the substrate; S4: inspect and dry the surface of the substrate after flocking.

[0015] Preferably, the high voltage value of the electric field of electrostatic flocking in step S3 is 80-90 kV.

[0016] Preferably, the drying temperature of the electrostatic flocking in step S4 is 20-40° C., and the drying time is 1-10 hours.

[0017] Beneficial effects of the present invention: 1. Preparation of two-component flocking interface glue: by mixing hydroxyl acrylic emulsion with water-based isocyanate, the hydroxyl group and the NCO group undergo polymerization to prepare the glue. Since the hydroxyl acrylic emulsion has good film-forming properties, weather resistance, acid resistance, alkali resistance, and improves the cross-linking density and adhesion of the paint film, the glue prepared by the emulsion can form an adhesive film with excellent water resistance and super strong adhesion. Then, a wetting agent is used to control its surface tension and increase the adhesion to the substrate. A cationic dispersant is used to better disperse the pigment, provide an anode electric field surface, prolong the open time of the two-component flocking interface glue film, and improve water resistance and adhesion.

[0018] 2. When the two-component flocking interface glue of the present invention is flocked, it can be extremely well adhered to the surface of various substrates to bond the fluff. The water resistance, weather resistance and aging resistance of the substrate surface after flocking are better than those of the existing flocking glue. The two-component flocking interface glue has a longer open time for film formation and can be suitable for large-area flocking scenes. The density of electrostatic flocking is higher, the bonded fluff is more, and the decorative effect is better. DETAILED DESCRIPTION

[0019] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0020] The present invention provides a two-component flocking interface adhesive, which is composed of a first component of glue and a second component of curing agent; The first component of glue comprises the following components and weight parts: 30-60 parts of hydroxy acrylic emulsion, 36.5-70 parts of hydroxyethyl cellulose aqueous solution, 0.1-0.5 parts of wetting agent, 0.1-0.5 parts of defoaming agent, and 0.3-0.5 parts of cationic dispersant; The second component curing agent includes the following ingredients and weight parts: 6-12 parts of water-based isocyanate and 1-3 parts of diethylene glycol butyl ether solvent; The solid content of the hydroxy acrylic emulsion is 42-48%, and the solid content of the water-based isocyanate is 80-100%.

[0021] The preparation of two-component flocking interface glue is achieved by mixing hydroxyl acrylic emulsion with water-based isocyanate to allow the hydroxyl group to undergo polymerization reaction with the NCO group. Since the hydroxyl acrylic emulsion has good film-forming properties, weather resistance, acid resistance, alkali resistance, and improves the cross-linking density and adhesion of the paint film, the glue prepared from it can form an adhesive film with excellent water resistance and super strong adhesion. A wetting agent is then used to control its surface tension and increase adhesion to the substrate. A cationic dispersant is used to better disperse the pigment, provide an anode electric field surface, extend the open time of the two-component flocking interface glue film, and improve water resistance and adhesion.

[0022] As a preferred embodiment of the present invention, the raw materials of the first component glue also include 1 to 2 parts by weight of pigment, and by adding the pigment, it is convenient to use the two-component flocking interface glue for flocking, and by observing the color, it is judged whether the two-component flocking interface glue sprayed or rolled has glue leakage, and at the same time, it has a color-changing effect on the covering, improves the covering rate of the fluff on the covering, and makes the color more uniform and beautiful; The hydroxylated acrylic emulsion includes a hydroxylated acrylic emulsion with the brand name of Double Bond Chemical DB3650; The wetting agent includes an ionic wetting agent or a non-ionic wetting agent, and the wetting agent includes a wetting agent with the brand name of Dow Chemical PE-100; The defoamer is an organosilicon defoamer, and the defoamer includes organosilicon defoamers with the brands of TEGO 901W and TEGO 902W; The cationic dispersant includes a cationic dispersant with the brand name of TEGO 690; The water-based isocyanate includes a water-based isocyanate with the brand name of Double Bond Chemical DB82547; The diethylene glycol butyl ether solvent includes diethylene glycol butyl ether solvents with the brands of DOW DB and DOW DOWANOL DBA.

[0023] There are certain restrictions on the amount of each raw material. The weight parts of hydroxyl acrylic emulsion include 30 parts, 32 parts, 34 parts, 36 parts, 38 parts, 40 parts, 42 parts, 44 parts, 46 parts, 48 ​​parts, 50 parts, 52 parts, 54 parts, 56 parts, 58 parts and 60 parts. If the amount of hydroxyl acrylic emulsion is too small (less than 30 parts), the organic molecular weight formed on the surface of the film will be reduced, which is not conducive to the bonding of the fluff during the flocking process. If the amount of hydroxyl acrylic emulsion is too large (higher than 60 parts), the production cost and the viscosity of the two-component flocking interface adhesive will increase, which is not conducive to construction.

[0024] The weight proportions of hydroxyethyl cellulose include 1 part, 2 parts and 3 parts. If the amount of hydroxyethyl cellulose is too little (less than 1 part), it is easy to cause the pigment stratification of the two-component flocking interface adhesive after preparation, which is not convenient for observation during construction. If the amount of hydroxyethyl cellulose is too much (higher than 3 parts), the viscosity of the prepared two-component flocking interface adhesive will be increased, making its fluidity poor and not conducive to construction.

[0025] The mass ratio of the hydroxy acrylic emulsion contained in the first component glue to the water-based isocyanate contained in the second component curing agent is 5:1.

[0026] As a preferred embodiment of the present invention, the hydroxyethyl cellulose aqueous solution comprises the following components and weight parts: 1 part of hydroxyethyl cellulose, 1 part of ammonia neutralizer and 98 parts of water, wherein the ammonia neutralizer comprises ammonia neutralizers of brands Henkel OP-10 and Dow AMP-95; The preparation method of the hydroxyethyl cellulose aqueous solution is as follows: 98 kg of water is added into a stirring kettle, the temperature of the stirring kettle is controlled to be 25° C., 1 kg of hydroxyethyl cellulose (30,000 molecular weight) is slowly added, and then 1 kg of ammonia neutralizer with the brand of Henkel OP-10 is added, the pH value of the hydroxyethyl cellulose aqueous solution is adjusted to 8, and the solution is dispersed at a high speed until no obvious particles are present, and then allowed to stand for 24 hours.

[0027] The present invention also provides a method for preparing the above two-component flocking interface adhesive, comprising the following steps: (a), mixing a hydroxy acrylic acid emulsion with a hydroxyethyl cellulose aqueous solution to obtain a mixture A; (b), mixing the wetting agent, the cationic dispersant and the defoaming agent with the mixture A to obtain a mixture B; (c) mixing the mixture B with the pigment to obtain a first component of glue; (d) mixing water-based isocyanate with diethylene glycol butyl ether solvent to obtain a second component curing agent; (e) Mix the first component glue and the second component curing agent to obtain a two-component flocking interface glue.

[0028] The first component glue and the second component curing agent are prepared by mixing the raw materials of the first component glue and the raw materials of the second component curing agent respectively, and then the first component glue and the second component curing agent are mixed and reacted, and static activation is performed to obtain a two-component flocking interface glue.

[0029] As a preferred embodiment of the present invention, the preparation mixing speed of the two-component flocking interface adhesive is 300~1500r / min, the reaction temperature is 10~40°C, in the step a, the reaction time is 5~10min, in the step b, the reaction time is 5~10min, in the step c, the reaction time is 20~30min, in the step d, the reaction time is 15~30min, and in the step e, the reaction time is 5~10min.

[0030] Specifically, if the preparation temperature of the two-component flocking interface adhesive is too low (≤10° C.), the mixing reaction time will be increased, affecting the efficiency; if the temperature is too high (≥40° C.), the hydroxylated acrylic emulsion will easily demulsify into a gelatinous substance.

[0031] As a preferred embodiment of the present invention, the room temperature viscosity of the two-component flocking interface adhesive is 200-300 KU.

[0032] As a preferred embodiment of the present invention, the facade flocking method comprises the following steps: S1: pre-treating the substrate surface; S2: Apply the two-component flocking interface adhesive to the surface of the substrate; S3: electrostatic flocking is performed on the surface of the substrate; S4: inspect and dry the surface of the substrate after flocking.

[0033] Specifically, the substrate includes interior walls, metal, glass, plastic and wood, etc.; the surface pretreatment of the interior wall includes hanging mesh leveling, sandpaper polishing and painting of acrylic emulsion primer, and the surface pretreatment of metal, glass, plastic, wood and other substrates includes cleaning the surface with a detergent and then polishing the surface oxide layer with sandpaper.

[0034] As a preferred embodiment of the present invention, the high voltage value of the electric field of electrostatic flocking in step S3 is 80-90 kV.

[0035] As a preferred embodiment of the present invention, the drying temperature of the electrostatic flocking in step S4 is 20-40° C., and the drying time is 1-10 hours.

[0036] The present invention will be further described below in conjunction with specific embodiments and comparative examples.

[0037] Example 1 In this embodiment, the following raw materials are prepared by weight: 30 kg of Double Bond Chemical DB3650 hydroxyl acrylic emulsion, 1 kg of pigment, 0.1 kg of Dow Chemical PE-100 wetting agent, 0.2 kg of TEGO 901W defoaming agent, 0.3 kg of TEGO 690 cationic dispersant, 68.4 kg of hydroxyethyl cellulose aqueous solution, 6 kg of Double Bond Chemical DB82547 water-based isocyanate, and 1 kg of DOW DB diethylene glycol butyl ether solvent.

[0038] The hydroxyethyl cellulose aqueous solution adopts the hydroxyethyl cellulose aqueous solution prepared as described above.

[0039] The preparation method of the two-component flocking interface adhesive comprises the following steps: Step (a): adding hydroxy acrylic acid emulsion and hydroxyethyl cellulose aqueous solution into a stirring tank 1, controlling the rotation speed of the stirring tank 1 to 1500 r / min, the temperature of the stirring tank 1 to 25° C., mixing and stirring for 10 minutes to obtain a mixture A; Step (b): adding a wetting agent, a cationic dispersant and a defoaming agent to the stirring tank one in sequence, mixing and reacting with the mixture A, controlling the rotation speed of the stirring tank one to be 300 r / min, mixing and stirring for 5 minutes, and obtaining a mixture B; Step (c): adding the pigment to the stirring tank 1 and mixing with the mixture B, controlling the rotation speed of the stirring tank 1 to 1500 r / min, mixing and stirring for 20 minutes, and preparing the first component glue; Step (d): adding aqueous isocyanate and diethylene glycol butyl ether solvent into a stirring kettle 2, controlling the rotation speed of the stirring kettle 2 to 300 r / min, the temperature of the stirring kettle 2 to 25° C., mixing and stirring for 15 minutes, and preparing a second component curing agent; Step (e): Add the prepared second component curing agent into the stirring kettle one, control the rotation speed of the stirring kettle one to 300 r / min, stir and mix for 5 minutes, and let it stand for activation for 3 minutes to prepare a two-component flocking interface adhesive.

[0040] When flocking is required, the prepared two-component flocking interface glue is sprayed or rolled onto the pretreated inner wall surface, and then the inner wall surface is flocked from bottom to top using flocking equipment to achieve vertical flocking of the inner wall surface. The electric field high voltage value of the electrostatic flocking is 90kv, the drying temperature of the inner wall surface after flocking is 25°C, and the drying time is 8h.

[0041] Example 2 In this embodiment, the following raw materials are prepared by weight: 60 kg of Double Bond Chemical DB3650 hydroxyl acrylic emulsion, 2 kg of pigment, 0.5 kg of Dow Chemical PE-100 wetting agent, 0.4 kg of TEGO 902W defoaming agent, 0.5 kg of TEGO 690 cationic dispersant, 36.6 kg of hydroxyethyl cellulose aqueous solution, 12 kg of Double Bond Chemical DB82547 water-based isocyanate, and 2 kg of Dow DOWANOLDBA diethylene glycol butyl ether solvent.

[0042] The hydroxyethyl cellulose aqueous solution adopts the hydroxyethyl cellulose aqueous solution prepared as described above.

[0043] The preparation method of the two-component flocking interface adhesive comprises the following steps: Step (a): adding hydroxy acrylic acid emulsion and hydroxyethyl cellulose aqueous solution into a stirring tank 1, controlling the rotation speed of the stirring tank 1 to 500 r / min, the temperature of the stirring tank 1 to 35° C., mixing and stirring for 5 minutes to obtain a mixture A; Step (b): adding a wetting agent, a cationic dispersant and a defoaming agent to the stirring tank one in sequence, mixing and reacting with the mixture A, controlling the rotation speed of the stirring tank one to be 300 r / min, mixing and stirring for 5 minutes, and obtaining a mixture B; Step (c): adding the pigment to the stirring kettle 1 and mixing with the mixture B, controlling the rotation speed of the stirring kettle 1 to 1500 r / min, mixing and stirring for 30 minutes, and preparing the first component glue; Step (d): adding aqueous isocyanate and diethylene glycol butyl ether solvent into a stirring kettle 2, controlling the rotation speed of the stirring kettle 2 to 300 r / min, the temperature of the stirring kettle 2 to 25° C., mixing and stirring for 30 minutes, and preparing a second component curing agent; Step (e): Add the prepared second component curing agent into the stirring kettle one, control the rotation speed of the stirring kettle one to 300 r / min, stir and mix for 5 minutes, and let it stand for activation for 3 minutes to obtain a two-component flocking interface adhesive.

[0044] When flocking is required, the two-component flocking interface glue is sprayed or rolled onto the pre-treated inner wall surface, and then the flocking equipment is used to perform flocking treatment on the inner wall surface from bottom to top to achieve vertical flocking of the inner wall surface. The electric field high voltage value of the electrostatic flocking is 85kv, the drying temperature of the inner wall surface after flocking is 30°C, and the drying time is 5h.

[0045] Example 3 In this embodiment, the following raw materials are prepared by weight: 40 kg of Double Bond Chemical DB3650 hydroxyl acrylic emulsion, 1.3 kg of pigment, 0.5 kg of Dow Chemical PE-100 wetting agent, 0.4 kg of TEGO 902W defoaming agent, 0.5 kg of TEGO 690 cationic dispersant, 57.3 kg of hydroxyethyl cellulose aqueous solution, 8 kg of Double Bond Chemical DB82547 water-based isocyanate, and 1 kg of DOW DB diethylene glycol butyl ether solvent.

[0046] The hydroxyethyl cellulose aqueous solution adopts the hydroxyethyl cellulose aqueous solution prepared as described above.

[0047] The preparation method of the two-component flocking interface adhesive comprises the following steps: Step (a): adding hydroxy acrylic acid emulsion and hydroxyethyl cellulose aqueous solution into a stirring tank 1, controlling the rotation speed of the stirring tank 1 to 500 r / min, the temperature of the stirring tank 1 to 30° C., mixing and stirring for 5 minutes to obtain a mixture A; Step (b): adding a wetting agent, a cationic dispersant and a defoaming agent to the stirring tank one in sequence, mixing and reacting with the mixture A, controlling the rotation speed of the stirring tank one to be 300 r / min, mixing and stirring for 5 minutes, and obtaining a mixture B; Step (c): adding the pigment to the stirring kettle 1 and mixing with the mixture B, controlling the rotation speed of the stirring kettle 1 to 1500 r / min, mixing and stirring for 30 minutes, and preparing the first component glue; Step (d): adding aqueous isocyanate and diethylene glycol butyl ether solvent into a stirring kettle 2, controlling the rotation speed of the stirring kettle 2 to 300 r / min, the temperature of the stirring kettle 2 to 30° C., mixing and stirring for 20 minutes, and preparing a second component curing agent; Step (e): Add the prepared second component curing agent into the stirring kettle one, control the rotation speed of the stirring kettle one to 300 r / min, stir and mix for 5 minutes, and let it stand for activation for 3 minutes to prepare a two-component flocking interface adhesive.

[0048] When flocking is required, the two-component flocking interface glue is sprayed or rolled onto the pre-treated inner wall surface, and then the flocking equipment is used to perform flocking treatment on the inner wall surface from bottom to top to achieve vertical flocking of the inner wall surface. The electric field high voltage value of the electrostatic flocking is 80kv, the drying temperature of the inner wall surface after flocking is 28°C, and the drying time is 4h.

[0049] Comparative Example 1 A comparative example of the two-component flocking interface adhesive of the present invention, the difference between this comparative example and Example 2 is only 80 parts of hydroxyl acrylic emulsion, 16.6 parts of hydroxyethyl cellulose aqueous solution, and 16 parts of aqueous isocyanate; the sources of other components and the preparation method and flocking method of the two-component flocking interface adhesive are the same as those of Example 2.

[0050] Comparative Example 2 A comparative example of the two-component flocking interface adhesive of the present invention, the difference between this comparative example and Example 2 is that the hydroxyl acrylic emulsion is replaced by an aqueous hydroxyl acrylic resin with a brand of Fuqisen AQUAPAC-8251, and the aqueous isocyanate is selected from the aqueous isocyanate with a brand of Fuqisen AQUAPU-379; the sources of the remaining components and the preparation method and flocking method of the two-component flocking interface adhesive are the same as those in Example 2.

[0051] Comparative Example 3 The existing polyvinyl alcohol glue is sprayed onto the pretreated inner wall surface, and then flocking treatment is performed on the inner wall surface from bottom to top using flocking equipment to achieve flocking on the inner wall surface. The high voltage value of the electric field of the electrostatic flocking is 85kv, the drying temperature of the inner wall surface after flocking is 25°C, and the drying time is 4h.

[0052] Comparative Example 4 The existing acrylic emulsion is sprayed onto the pretreated inner wall surface, and then flocking treatment is performed on the inner wall surface from bottom to top using flocking equipment to achieve flocking on the inner wall surface. The electric field high voltage value of the electrostatic flocking is 85kv, the drying temperature of the substrate surface after flocking is 25°C, and the drying time is 5h.

[0053] Quality comparison: Example 1, Example 2, Example 3 and Comparative Example 1, Comparative Example 2 and the existing flocking adhesive were compared in flocking the inner wall surface according to the application process (as shown in Table 1): Table 1 It can be seen from Table 1 that when the two-component flocking interface adhesive of the present invention is used for flocking, when the various embodiments of the present invention are used to flock the wall, the overall performance is better than the control example, and with the increase in the mass fraction of hydroxyl acrylic emulsion, the organic molecular weight formed on the surface of the film increases, which is beneficial to the bonding of the fluff during the flocking process, so that the various performances of the two-component flocking interface adhesive are gradually enhanced. When the mass fraction of hydroxyl acrylic emulsion exceeds 60 parts, the various performances of the prepared two-component flocking interface adhesive remain unchanged, and the production cost and the viscosity of the two-component flocking interface adhesive will be increased, which is not conducive to construction. Therefore, Example 2 is the optimal ratio of the raw materials of the two-component flocking interface adhesive of the present invention, with low production cost, easy construction, and is beneficial to adhesion to various substrate surfaces and bonding fluff. The flocking density is higher, the fluff is more bonded, and the decorative effect is better.

[0054] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modification, equivalent substitution or improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A two-component flocking interface adhesive, characterized in that; The two-component flocking interface glue is composed of a first component of glue and a second component of curing agent; The first component of glue comprises the following components and weight parts: 30-60 parts of hydroxy acrylic emulsion, 36.5-70 parts of hydroxyethyl cellulose aqueous solution, 0.1-0.5 parts of wetting agent, 0.1-0.5 parts of defoaming agent, and 0.3-0.5 parts of cationic dispersant; The second component curing agent includes the following ingredients and weight parts: 6-12 parts of water-based isocyanate and 1-3 parts of diethylene glycol butyl ether solvent; The solid content of the hydroxy acrylic emulsion is 42-48%, and the solid content of the water-based isocyanate is 80-100%.

2. A two-component flocking interface adhesive according to claim 1, characterized in that: The raw materials of the first component glue also include 1 to 2 parts by weight of pigment; The hydroxylated acrylic emulsion includes a hydroxylated acrylic emulsion with the brand name of Double Bond Chemical DB3650; The wetting agent is a cationic wetting agent or a nonionic wetting agent; The defoamer is an organosilicon defoamer; The cationic dispersant includes a cationic dispersant with the brand name of TEGO 690; The water-based isocyanate includes a water-based isocyanate with the brand name of Double Bond Chemical DB82547; The diethylene glycol butyl ether solvent includes diethylene glycol butyl ether solvents with the brands of DOW DB and DOW DOWANOL DBA.

3. The two-component flocking interface adhesive according to claim 1, characterized in that: The mass ratio of the hydroxy acrylic emulsion contained in the first component glue to the water-based isocyanate contained in the second component curing agent is 5:

1.

4. The two-component flocking interface adhesive according to claim 1, characterized in that: The hydroxyethyl cellulose aqueous solution comprises the following components and weight parts: 1-3 parts of hydroxyethyl cellulose, 1-3 parts of ammonia neutralizer, and 96-98 parts of water; The ammonia neutralizer includes Henkel OP-10 and Dow AMP-95. The hydroxyethyl cellulose and the ammonia neutralizer are mixed with water to obtain a hydroxyethyl cellulose aqueous solution.

5. A two-component flocking interface adhesive according to claim 4, characterized in that: The pH value of the hydroxyethyl cellulose aqueous solution is 8-9, the reaction temperature for preparing the hydroxyethyl cellulose aqueous solution is 10-40° C., and the reaction time is 12-36 hours.

6. A method for preparing a two-component flocking interface adhesive according to any one of claims 1 to 5, characterized in that: The preparation method comprises the following steps: Mixing a hydroxy acrylic acid emulsion with a hydroxyethyl cellulose aqueous solution to obtain a mixture A; mixing a wetting agent, a cationic dispersant and a defoaming agent with mixture A to obtain mixture B; Mixing mixture B with the pigment to obtain a first component of glue; Mixing water-based isocyanate with diethylene glycol butyl ether solvent to obtain a second component curing agent; The first component of glue and the second component of curing agent are mixed to obtain a two-component flocking interface adhesive.

7. The method for preparing a two-component flocking interface adhesive according to claim 6, characterized in that: The preparation mixing speed of the two-component flocking interface adhesive is 300~1500r / min, the mixing reaction temperature is 10~40°C, the reaction time in step a is 5~10min, the reaction time in step b is 5~10min, the reaction time in step c is 20~30min, the reaction time in step d is 15~30min, and the reaction time in step e is 5~10min.

8. The method for preparing a two-component flocking interface adhesive according to claim 6, characterized in that: The room temperature viscosity of the two-component flocking interface adhesive is 200-300 KU.

9. A vertical flocking method of a two-component flocking interface adhesive according to claims 1 to 5, characterized in that: The facade flocking method comprises the following steps: S1: pre-treating the substrate surface; S2: Apply the two-component flocking interface adhesive to the surface of the substrate; S3: electrostatic flocking is performed on the surface of the substrate; S4: inspect and dry the surface of the substrate after flocking.

10. The vertical surface flocking method of the two-component flocking interface adhesive according to claim 9, characterized in that: The electric field high voltage value of the electrostatic flocking in step S3 is 80-90 kV, and the drying temperature after flocking in step S4 is 20-40° C., and the drying time is 1-10 hours.

Citation Information