Composite phase change material as well as preparation method and application thereof

By adding Al2O3 nanoparticles to sodium acetate trihydrate to form a composite phase change material, the problem of low thermal conductivity of existing phase change materials is solved, and higher thermal conductivity and broader application prospects are achieved.

CN118909596APending Publication Date: 2024-11-08BEIJING GUODIAN FUTONG SCI & TECH DEV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410869739.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-01
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The low thermal conductivity of existing phase change materials limits their energy storage efficiency and is difficult to meet the efficient heat transfer needs in areas such as energy, construction and aerospace.

Method used

By combining 0.05% to 0.1% of Al2O3 nanoparticles (particle size 5-15nm) with sodium acetate trihydrate, a composite phase change material is formed to improve its thermal conductivity, and a preparation method of mixing and tableting is adopted.

Benefits of technology

The thermal conductivity of composite phase change materials has been significantly improved, making them suitable for heat storage devices such as wall insulation, solar power plants and aerospace equipment, and improved resource utilization and application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118909596A_ABST
    Figure CN118909596A_ABST
Patent Text Reader

Abstract

The invention discloses a composite phase change material and a preparation method and application thereof. The composite phase change material comprises 99.9%-99.95% of an energy storage main body material and 0.05%-0.1% of a thermal conductivity regulator, the energy storage main body material is sodium acetate trihydrate, and the thermal conductivity regulator is Al2O3; the preparation method comprises the following steps: mixing sodium acetate trihydrate and Al2O3 nanoparticles, and tabletting. Compared with pure sodium acetate trihydrate, the composite phase change material disclosed by the invention has higher heat conductivity, can be applied to the aspects of wall insulation, solar power stations, aerospace equipment and the like, and has a wide application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a phase change material and a preparation method and application thereof, and in particular to a composite phase change material and a preparation method and application thereof. Background Art

[0002] As energy shortage and environmental pollution become increasingly prominent, people attach more and more importance to improving resource utilization. Energy storage technology is an important method to solve the imbalance between energy supply and demand, and has attracted much attention from domestic researchers. Phase change energy storage technology refers to the use of phase change energy storage materials to undergo phase change at a certain temperature, absorb or release heat energy to adjust the temperature of the environment. Phase change energy storage materials refer to substances that have the characteristics of phase change within a certain temperature range. When the temperature rises, they absorb the heat energy in the environment, undergo phase change, and convert it into their own phase change enthalpy for storage; when the temperature drops, they undergo reverse phase change and release the heat, but their own temperature does not change. It shows considerable development potential in the fields of energy, construction, aerospace, chemical industry, etc. Thermal conductivity is one of the important physical parameters of phase change materials. It determines the speed of heat transfer of materials. Higher thermal conductivity can improve the efficiency of material energy storage. How to improve the thermal conductivity of traditional phase change materials is a technical problem that needs to be solved at present. Summary of the invention

[0003] Purpose of the invention: The present invention aims to provide a composite phase change material with high thermal conductivity; the present invention also aims to provide a method for preparing the composite phase change material; another purpose of the present invention is to provide an application of the composite phase change material.

[0004] Technical solution: The composite phase change material of the present invention comprises, by mass percentage:

[0005] Energy storage main material 99.9%~99.95%,

[0006] Thermal conductivity regulator 0.05% to 0.1%,

[0007] The energy storage main material is sodium acetate trihydrate, and the thermal conductivity regulator is Al2O3.

[0008] Preferably, the thermal conductivity regulator is Al2O3 nanoparticles with a particle size of 5-15 nm, and the thermal conductivity of the composite phase change material is higher than that of the pure energy storage main material.

[0009] The preparation method of the composite phase-change energy storage material comprises: mixing and tableting the energy storage main material and the thermal conductivity regulator.

[0010] Preferably, during the mixing process, the energy storage main material and the thermal conductivity regulator are added into a mixing device, and mixed and stirred for 30-60 minutes.

[0011] Preferably, during the tableting process, the stirred and mixed materials are added into a tableting device and then tableted.

[0012] The composite phase change material can be used in a heat storage device.

[0013] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages: the composite phase change material has higher thermal conductivity than pure sodium acetate trihydrate, can be applied to heat storage devices such as wall insulation, solar power stations, aerospace equipment, etc., and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 It is a test diagram of the phase change temperature and phase change latent heat of the composite phase change material energy storage main material of the present invention;

[0015] Figure 2 This is a physical picture of the composite phase change material sample obtained in the comparative example;

[0016] Figure 3 This is a physical picture of the composite phase change material sample obtained in Example 1. DETAILED DESCRIPTION

[0017] The technical solution of the present invention is further described below in conjunction with the accompanying drawings.

[0018] Example 1

[0019] The composite phase change material of this embodiment includes (by mass percentage):

[0020] Composite phase change material energy storage main material 99.95%;

[0021] Thermal conductivity regulator 0.05%;

[0022] The main energy storage material of the composite phase change material is sodium acetate trihydrate, and the thermal conductivity regulator is Al2O3 nanoparticles with a particle size of 10nm.

[0023] Example 2

[0024] The composite phase change material of this embodiment includes (by mass percentage):

[0025] Composite phase change material energy storage main material 99.9%;

[0026] Thermal conductivity regulator 0.1%;

[0027] The main energy storage material of the composite phase change material is sodium acetate trihydrate, and the thermal conductivity regulator is Al2O3 nanoparticles with a particle size of 10nm.

[0028] The manufacturing method of the composite phase change energy storage material comprises:

[0029] Step 1: Mixing process of composite phase change materials

[0030] Step 2: The tableting process of composite phase change materials

[0031] During the mixing process of the composite phase change material, a certain mass of the energy storage main material and the thermal conductivity regulator are weighed and added to the mixing device, and the mixture is mixed and stirred for 30 minutes; during the tableting process of the composite phase change material, the mixed material is added to the tableting device, and then tableted.

[0032] Comparative Example

[0033] The composite phase change material of this comparative example includes (by mass percentage):

[0034] Composite phase change material energy storage main material 100%;

[0035] Thermal conductivity regulator 0%;

[0036] The main material of the composite phase change material energy storage is sodium acetate trihydrate.

[0037] The thermal conductivity, density and specific heat capacity corresponding to the composite phase change materials of Examples 1-2 and the comparative example are shown in Table 1.

[0038] Table 1 Thermal conductivity, density and specific heat capacity of composite phase change materials

[0039] Thermal conductivity W / mK Specific heat capacity KJ / kg3K Comparative Example 2.052 1.9 Example 1 2.134 1.8994 Example 2 2.212 1.8989

Claims

1. A composite phase change material, characterized in that: Included by mass percentage: Energy storage main material 99.9%~99.95%, Thermal conductivity regulator 0.05% to 0.1%, The energy storage main material is sodium acetate trihydrate, and the thermal conductivity regulator is Al2O3.

2. The composite phase change material according to claim 1, characterized in that: The thermal conductivity regulator is Al2O3 nanoparticles.

3. The composite phase change material according to claim 1, characterized in that: The particle size of the Al2O3 nanoparticles is 5-15nm.

4. The composite phase change material according to claim 1, characterized in that: The thermal conductivity of the composite phase change material is higher than that of the pure energy storage main material.

5. A method for preparing the composite phase change energy storage material according to any one of claims 1 to 4, characterized in that: The method comprises: mixing and tableting an energy storage main body material and a thermal conductivity regulator.

6. The method for preparing the composite phase change energy storage material according to claim 5, characterized in that: During the mixing process, the energy storage main material and the thermal conductivity regulator are added into a mixing device and mixed and stirred.

7. The method for preparing the composite phase change energy storage material according to claim 6, characterized in that: The mixing time is 30-60 minutes.

8. The method for preparing the composite phase change energy storage material according to claim 5, characterized in that: During the tableting process, the stirred and mixed materials are added to the tableting device and then tableted.

9. The method for preparing the composite phase change energy storage material according to claim 5, characterized in that: During the tableting process of the composite phase change material, the applied pressure is 8-12MPa.

10. Use of the composite phase change material according to any one of claims 1 to 4 in a heat storage device.