Efficient production method of high-aluminum non-magnetic steel

By using deep deoxygenation and electromanganese alloys in the production process of high-aluminum magnet-free steel, combined with the addition of aluminum ingots and manganese elements at one time, the problems of difficulty in component control and low production efficiency are solved, and efficient production and high purity are achieved. Finished product.

CN118910363APending Publication Date: 2024-11-08FUSTEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410985652.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the production process of existing high-aluminum magnetic steel, due to the high content of Mn and Al elements and the difficulty of controlling components, there are many uncontrollable factors, low production efficiency, low alloy yield and decreased purity during the smelting process.

Method used

Deep deoxygenation and electromanganese are used as manganese-enhancing alloys to reduce uncontrollable factors, and aluminium ingots and manganese elements are added at one time during the electric furnace and LF refining process to control the composition of the molten steel, shorten the smelting time, and improve production efficiency and purity.

Benefits of technology

Improve the production efficiency and alloy yield of high-aluminum magnetic steel, enhance the purity of the finished product, shorten the smelting time of electric furnace to 2.5-3 hours, shorten the LF refining time to 60-90 minutes, and increase the yield of aluminum ingots to More than 86.6%.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses an efficient production method of high-aluminum non-magnetic steel, which comprises the following steps: a, adding carbon steel into an electric furnace, blowing carbon to less than or equal to 0.10%, dephosphorizing to less than or equal to 0.020%, and flowing slag to obtain a product A, b, adding aluminum ingots into each ton of the product A, and carrying out deep deoxidation to obtain a product B, c, adding electric manganese into the product B, controlling the Mn content in molten steel to be 18-22%, heating and tapping to obtain a product C, and d, tapping the product C to an LF furnace for refining, adding lime, fluorite and refining slag into the product C until the slag is white, adjusting the Al content of the molten steel, and adjusting the manganese element content to a target value at one time according to the Mn element content of the molten steel to obtain a product D, and e, adding an aluminum ingot according to the aluminum content in the product D, adjusting the aluminum element content to a target value at one time to obtain a product E, heating the product E, and carrying out crane ladle pouring to obtain a finished product. The method has the advantage of high production efficiency, the alloy yield is high, and the purity of a finished product is further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of high-aluminum non-magnetic steel, and in particular relates to a high-efficiency production method of high-aluminum non-magnetic steel. Background Art

[0002] 18Mn25AlV type high aluminum non-magnetic steel (C: 0.14-0.22%, Mn: 20.5-25.0%, Al: 1.50-2.50%, V: 0.04-0.30%, Si≤1.0%, P≤0.030%, S≤0.030%), since the Mn content of this steel is as high as 20.5-25.0%, which is much higher than that of conventional steel (the Mn content of conventional steel is less than 2.0%), so the composition control is more difficult, and the alloy used to increase manganese in the production process is used. The amount of manganese is large, and the content of elements other than Mn in the manganese-enhanced alloy will lead to a high content of carbon and other elements at the same time as the manganese is increased, which will cause uncontrollable factors in the smelting process. Therefore, the selection of the type of manganese alloy is also very demanding; the Al content of the steel grade is as high as 1.50-2.50%, and the aluminum element in high-aluminum steel is extremely easy to oxidize in the molten steel, which makes the Al element composition fluctuate greatly during the smelting process, the aluminum ingot yield is low, and the large amount of Al2O3 produced will cause the purity of the molten steel to decrease, which makes the composition control of the smelting process extremely difficult. In the smelting process, in order to accurately control the composition content of the molten steel, a multi-batch alloy addition mode is adopted. The electric furnace smelting time is 4-6 hours, the smelting cycle is long, and the production efficiency is low. Therefore, the existing high-aluminum non-magnetic steel has the defect of low production efficiency. Summary of the Invention

[0003] The object of the present invention is to provide a highly efficient method for producing high-aluminum non-magnetic steel. The present invention has the advantages of high production efficiency and high alloy yield, thereby improving the purity of the finished product.

[0004] The technical solution of the present invention is: a high-efficiency production method of high-aluminum non-magnetic steel, comprising the following steps:

[0005] a. Add carbon steel into the electric furnace, blow carbon to ≤0.10%, dephosphorize to ≤0.020%, flow slag, and get Grade A.

[0006] b. Add 9-15 kg of aluminum ingots to each ton of product A and perform deep deoxidation. The aluminum content in the molten steel after deep deoxidation is > 0.10%, and product B is obtained.

[0007] c. Add 180-250 kg of electromanganese per ton of product B, control the Mn content in the molten steel to 18-22%, heat it to 1640-1660°C, tap it, and get product C.

[0008] d. Product C is tapped and sent to the LF furnace for refining. During refining, 15-25kg of lime, 10-15kg of fluorite, and 3.5-6kg of refining slag are added to each ton of product C until the slag turns white. The Al content of the molten steel is adjusted to > 0.10%. According to the Mn content of the molten steel, the manganese content is adjusted to the target value at one time to obtain product D.

[0009] e. According to the aluminum content in product D, add aluminum ingots and adjust the aluminum content to the target value at one time to obtain product E. Heat product E to 1500-1520℃ and ladle pouring to obtain the finished product.

[0010] In the aforementioned high-efficiency production method of high-aluminum non-magnetic steel, in step a, carbon is blown to 0.05% and dephosphorization is performed to 0.019%.

[0011] In the aforementioned efficient production method of high-aluminum non-magnetic steel, in step b, 10.3 kg of aluminum ingots are added to each ton of product A, and the aluminum content in the molten steel after deep deoxidation is 0.2%.

[0012] In the aforementioned high-efficiency production method of high-aluminum non-magnetic steel, in step c, 210 kg of electromanganese is added to each ton of product B, the Mn content in the molten steel is controlled at 19.4%, and the temperature is raised to 1650°C.

[0013] In the aforementioned efficient production method of high-aluminum non-magnetic steel, the electric furnace smelting time is 2.5-3 hours.

[0014] In the aforementioned efficient production method of high-aluminum non-magnetic steel, the electric furnace smelting time is 2.75 hours, the smelting time in step a accounts for about 50%, the smelting time in step b accounts for about 20%, and the smelting time in step c accounts for about 30%.

[0015] In the aforementioned efficient production method of high-aluminum non-magnetic steel, in step d, 20 kg of lime, 12.5 kg of fluorite, and 4.4 kg of refined slag are added to each ton of product C.

[0016] In the aforementioned high-efficiency production method of high-aluminum non-magnetic steel, in step e, 16.3 kg of aluminum ingots are added to each ton of product D to adjust the aluminum content to 1.68%.

[0017] In the aforementioned efficient production method of high-aluminum non-magnetic steel, the LF furnace refining time is 60-90 minutes.

[0018] In the aforementioned high-efficiency production method of high-aluminum non-magnetic steel, the LF furnace refining time is 80 minutes, the smelting time in step d accounts for 70%, and the smelting time in step e accounts for 30%.

[0019] Compared with the prior art, the present invention performs deep deoxidation in the furnace by adding a sufficient amount of aluminum ingots after oxygen blowing, dephosphorization and decarburization in the electric furnace, and adopts electric manganese (electrolytic manganese) as the manganese alloy for increasing manganese. The manganese alloy does not contain other components, which reduces uncontrollable factors, so that the manganese alloy can be added all at once during electric furnace smelting, thereby reducing the smelting waiting time caused by sampling and chemical processing after each addition, improving production efficiency, and also improving the yield of the alloy.

[0020] Based on the use of electromanganese as the manganese-increasing alloy and the reduction of uncontrollable factors, aluminum only needs to be added twice, which can reduce the smelting waiting time caused by sampling and chemical processing after each addition, improve production efficiency and also increase the aluminum ingot yield.

[0021] By analyzing the characteristics that multiple additions of aluminum easily lead to long smelting time and aluminum in molten steel is easily oxidized during this process, a material addition method of deep deoxidation in the early stage of LF refining and adding aluminum ingots in the middle and late stages of LF refining is adopted to reduce the oxidation of aluminum in molten steel, reduce the fluctuation of Al element composition in the smelting process, improve the aluminum ingot yield, avoid the generation of a large amount of Al2O3, and improve the purity of molten steel, that is, improve the purity of the finished product.

[0022] Therefore, the present invention has the advantages of high production efficiency and high alloy yield, thereby improving the purity of the finished product. DETAILED DESCRIPTION

[0023] The present invention will be further described below with reference to the examples, but they are not intended to limit the present invention.

[0024] Example 1. An efficient production method for high-aluminum non-magnetic steel, comprising the following steps:

[0025] a. Add carbon steel into the electric furnace, blow carbon to 0.05%, dephosphorize to 0.019%, flow slag, and obtain Grade A.

[0026] b. Add 10.3 kg of aluminum ingots to each ton of product A and perform deep deoxidation. The aluminum content in the molten steel after deep deoxidation is 0.2%, and product B is obtained.

[0027] c. Add 210 kg of electrolytic manganese per ton of product B, adjust the Mn content in the molten steel to 19.4%, energize the electric furnace, heat the steel to 1650°C, and tap the steel to obtain product C. In step c, 210 kg of electrolytic manganese is added all at once after deep deoxidation of the molten steel. This significantly improves the electrolytic manganese yield compared to the batch addition method (three or more times) in existing production methods. With the existing feeding method, the electrolytic manganese yield is only 65-75%.

[0028] Steps a to c above represent the electric furnace smelting stage, wherein step a accounts for approximately 50% of the smelting time, step b accounts for approximately 20% of the smelting time, and step c accounts for approximately 30% of the smelting time. The total smelting time is 2 hours and 45 minutes, and the electrolytic manganese yield is 93%. The operation of steps a to c can reduce the frequency of sampling and material processing, shorten the smelting waiting time, and reduce the electric furnace smelting time from 4-6 hours to less than 3 hours, greatly improving the efficiency of the electric furnace smelting stage.

[0029] d. Product C is tapped and sent to the LF furnace for refining. During refining, 20kg of lime, 12.5kg of fluorite, and 4.4kg of refining slag are added to each ton of product C until the slag turns white. The Al content of the molten steel is adjusted to > 0.10%. Based on the Mn content of the molten steel, the manganese content is adjusted to the target value at one time to obtain product D.

[0030] e. According to the aluminum content in product D, add aluminum ingots, adding 16.3 kg of aluminum ingots to each ton of product D, and adjust the aluminum content to the target value of 1.68%. Add ferrovanadium at a rate of 1.5 kg per ton of steel to ensure that the vanadium content meets the standard. Product E is obtained. The temperature of product E is raised to 1500-1520 ° C to meet the casting conditions, and the product is cast by hanging ladle casting to obtain the finished product.

[0031] Steps d and e are the LF refining stage. Step d accounts for 70% of the smelting time, while step e accounts for 30% of the smelting time. The total refining time is 80 minutes, and the aluminum ingot yield is 86.6%. The LF refining stage can shorten the original LF refining time from >150 minutes to 60-90 minutes, and increase the LF refining aluminum ingot yield from 60-70% to over 80%.

[0032] Example 2:

[0033] 1) The electric furnace uses high-quality carbon steel as raw material, blows carbon to 0.13%, and dephosphorizes to 0.007%;

[0034] 2) After the slag is removed from the electric furnace, add 13kg of aluminum ingots per ton of steel and adjust the aluminum content to 0.13%;

[0035] 3) Add 245kg / ton of steel electric manganese, adjust the Mn element composition to 20.8, and heat the material to 1650℃, then tap the steel;

[0036] 4) The total smelting time in the electric furnace is 2h15min, and the electric manganese yield is 85%;

[0037] 5) The molten steel is put into LF refining, and lime, fluorite and 5.0 kg / ton of refined slag are added to make slag. After the slag turns white, the Al content is adjusted to 0.38%, and the one-time addition amount of electric manganese is calculated to adjust the Mn element content to the target value;

[0038] 6) Add 18.5kg of aluminum ingot per ton of steel to adjust the Al content to 1.83%, and add 1.5kg of ferrovanadium per ton of steel to adjust the V content;

[0039] 7) Adjust the temperature to meet the pouring conditions and then pour by ladle. The LF refining time is 62 minutes and the aluminum ingot yield is 86.8%.

[0040] In Example 2, the amount of each raw material and auxiliary material added is calculated based on tons of steel, that is, the amount required to be added when smelting one ton of finished product is calculated.

Claims

1. An efficient production method for high-aluminum non-magnetic steel, characterized in that: The following steps are included: a. Add carbon steel into the electric furnace, blow carbon to ≤0.10%, dephosphorize to ≤0.020%, drain slag, and get Grade A. b. Add 9-11 kg aluminum ingots to each ton of product A for deep deoxidation. The aluminum content in the molten steel after deep deoxidation is > 0.10%, and product B is obtained. c. Add 180-250 kg of electric manganese to each ton of product B, control the Mn content in the molten steel to 18-22%, raise the temperature to 1640-1660°C, tap the steel, and obtain product C. d. Product C is sent to LF furnace for refining. During refining, 15-25kg of lime, 10-15kg of fluorite and 3.5-6kg of refining slag are added to each ton of product C until the slag becomes white. The Al content of the molten steel is adjusted to > 0.10%. According to the Mn content of the molten steel, the manganese content is adjusted to the target value at one time to obtain product D. e. According to the aluminum content in product D, add aluminum ingots and adjust the aluminum content to the target value at one time to obtain product E. Product E is heated to 1500-1520℃ and cast by ladle to obtain the finished product.

2. The high-efficiency production method of high-aluminum non-magnetic steel according to claim 1 is characterized in that: In the step a, carbon is blown to 0.05% and dephosphorization is performed to 0.019%.

3. The high-efficiency production method of high-aluminum non-magnetic steel according to claim 1 is characterized in that: In the step b, 10.3 kg of aluminum ingots are added to each ton of product A, and the aluminum content in the molten steel after deep deoxidation is 0.2%. 。 4. The high-efficiency production method of high-aluminum non-magnetic steel according to claim 1 is characterized in that: In the step c, 210 kg of electromanganese is added to each ton of product B, the Mn content in the molten steel is controlled at 19.4%, and the temperature is raised to 1650°C.

5. The high-efficiency production method of high-aluminum non-magnetic steel according to claim 1 is characterized in that: Electric furnace smelting time is 2.5-3h.

6. The high-efficiency production method of high-aluminum non-magnetic steel according to claim 5, characterized in that: The electric furnace smelting time is 2.75h, of which the smelting time in step a accounts for about 50%, the smelting time in step b accounts for about 20%, and the smelting time in step c accounts for about 30%.

7. The high-efficiency production method of high-aluminum non-magnetic steel according to claim 1 is characterized in that: In the step d, 20 kg of lime, 12.5 kg of fluorite and 4.4 kg of refined slag are added to each ton of product C.

8. The high-efficiency production method of high-aluminum non-magnetic steel according to claim 1 is characterized in that: In the step e, 16.3 kg of aluminum ingots are added to each ton of product D to adjust the aluminum content to 1.68%.

9. The high-efficiency production method of high-aluminum non-magnetic steel according to claim 1 is characterized in that: LF furnace refining time is 60-90min.

10. The high-efficiency production method of high-aluminum non-magnetic steel according to claim 9, characterized in that: The LF furnace refining time is 80 minutes. The smelting time in step d accounts for 70%, and the smelting time in step e accounts for 30%.