Preparation method for liquid quenching treatment of high-hardness steel balls

By using aqueous quenching media of polyalkylene glycol and polyvinylpyrrolidone and reasonable alloy formula in the preparation process of high-carbon steel balls, the problems of uneven stress distribution and uneven carbide distribution of high-carbon steel balls are solved, and the problem of uneven stress distribution of high-carbon steel balls is achieved. It improves toughness and hardness, avoids cracking and improves yield.

CN118910368APending Publication Date: 2024-11-08CNBM NINGGUO XINMA WEAR RESISTANT MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410990729.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

During the preparation process, high-carbon steel balls are prone to cracking due to uneven stress distribution and uneven carbide distribution, which reduces the yield rate.

Method used

Use an aqueous solution containing polyalkane glycol and polyvinylpyrrolidone as the quenching medium, and use its molecular weight and content to reasonably adjust its molecular weight and content, and combine the C, Cr and V content in the alloy formula to perform austenitization and tempering treatment to control quenching. Stress distribution and carbide refinement during the process.

Benefits of technology

It effectively avoids quenching and cracking of steel balls, improves the toughness and hardness of steel balls, and improves the yield rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004958796320000051
    Figure BDA0004958796320000051
  • Figure BDA0004958796320000061
    Figure BDA0004958796320000061
Patent Text Reader

Abstract

The invention discloses a preparation method of a liquid-quenched high-hardness steel ball, which comprises the following steps: austenitizing a high-carbon steel ball blank, and then quenching and tempering to obtain the high-hardness steel ball, wherein the quenching medium is an aqueous solution containing polyalkylene glycol and polyvinylpyrrolidone. The toughness and hardness of the steel balls can be improved, cracking of the steel balls is avoided, and the yield of steel ball preparation is increased.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of alloy steel, and in particular to a method for preparing a liquid quenching treated high-hardness steel ball. Background Art

[0002] High carbon steel balls have high hardness and wear resistance and can be used as wear-resistant steel balls. However, when preparing high carbon steel balls, the high content of carbon elements will form hard and brittle carbides, and there is often a problem of uneven distribution of carbides; and during quenching, high carbon steel balls will have uneven stress distribution problems, which will cause high carbon steel balls to crack easily during the preparation process, reducing the yield rate of high carbon steel balls. Summary of the invention

[0003] Based on the technical problems existing in the background technology, the present invention proposes a method for preparing a high-hardness steel ball through liquid quenching treatment; the present invention can improve the toughness and hardness of the steel ball, avoid cracking of the steel ball, and improve the yield rate of steel ball preparation.

[0004] The invention provides a method for preparing a high-hardness steel ball by liquid quenching treatment, comprising the following steps: taking a high-carbon steel ball blank for austenitization treatment, and then quenching and tempering to obtain a high-hardness steel ball; wherein the quenching medium is an aqueous solution containing polyalkylene glycol and polyvinyl pyrrolidone.

[0005] Preferably, in the quenching medium, the mass fraction of polyalkylene glycol is 6-8wt%, and the mass fraction of polyvinyl pyrrolidone is 0.6-0.8wt%.

[0006] Preferably, the average molecular weight of the polyalkylene glycol is 20,000-25,000.

[0007] Preferably, the polyvinyl pyrrolidone consists of polyvinyl pyrrolidone with an average molecular weight of 1,400,000-1,600,000 and polyvinyl pyrrolidone with an average molecular weight of 40,000-50,000.

[0008] Preferably, the weight ratio of polyvinyl pyrrolidone with an average molecular weight of 1,400,000-1,500,000 to polyvinyl pyrrolidone with an average molecular weight of 40,000-50,000 is 3-4:1.

[0009] Preferably, the temperature of the quenching medium is 30-40°C.

[0010] Preferably, the raw materials of the high carbon steel ball blank include, by weight percentage: C 0.9-1.1%, Cr 6-8%, Mo0.3-0.35%, V 0.35-0.4%, and the balance is Fe and inevitable impurities.

[0011] Preferably, the raw materials of the high carbon steel ball blank include, by weight percentage: C 1.0%, Cr 7%, Mo 0.3%, V 0.38%, and the balance is Fe and inevitable impurities.

[0012] Preferably, the austenitizing temperature is 990-1100° C. and the time is 2-3 h.

[0013] Preferably, the tempering temperature is 190-210° C. and the tempering time is 3-5 h.

[0014] Preferably, after tempering, the steel is air-cooled to room temperature.

[0015] Beneficial effects:

[0016] The present invention aims at the problems of uneven stress distribution, easy cracking and low toughness of high carbon steel balls during quenching. Polyalkylene glycol and polyvinyl pyrrolidone with suitable molecular weight are selected to cooperate with each other as quenching medium, and their content is adjusted so that the quenching medium has a fast cooling speed at high temperature, promotes austenite transformation, and reduces the cooling speed at low temperature, so that in the martensite transformation stage, the stress is reduced and the stress distribution is uniform, so as to avoid quenching cracking of the steel ball and maintain good hardness.

[0017] In addition, by designing a suitable alloy formula and adjusting the contents of C, Cr and V, the alloy has good hardenability, which can further reduce stress during quenching and make the stress distribution uniform to avoid cracking; in addition, the appropriate amount of V and C content can consume C elements to form carbides, refine carbides, make them evenly distributed, and hinder dislocation movement and refine martensite, thereby improving the toughness of the steel ball while maintaining a high hardness;

[0018] In addition, the present invention performs tempering at an appropriate temperature to further improve the hardness of the steel ball; the present invention makes the steel ball have high hardness while maintaining good toughness through the mutual coordination of the steel ball formula, quenching medium and heat treatment process, and avoids the problem of easy quenching cracking of the steel ball, thereby improving the yield rate of high carbon steel balls. DETAILED DESCRIPTION

[0019] The technical solution of the present invention is described in detail below through specific embodiments.

[0020] Example 1

[0021] A preparation method of a high-hardness steel ball by liquid quenching, comprising the following steps: taking a high-carbon steel ball blank, first heating it to 650°C, keeping it warm for 1 hour, then heating it to 880°C, keeping it warm for 1 hour, then heating it to 990°C, keeping it warm for 3 hours to perform austenitization treatment, then adding it to a quenching medium at a temperature of 40°C, quenching it until the surface temperature of the high-carbon steel ball is the same as the temperature of the quenching medium, then taking it out, tempering it in a tempering furnace at 190°C for 5 hours, taking it out, and air cooling it to room temperature to obtain a high-hardness steel ball;

[0022] Wherein, the quenching medium is an aqueous solution containing 6wt% polyalkylene glycol and 0.6wt% polyvinyl pyrrolidone;

[0023] The average molecular weight of polyalkylene glycol is 20,000;

[0024] The polyvinyl pyrrolidone is composed of polyvinyl pyrrolidone with an average molecular weight of 1,600,000 and polyvinyl pyrrolidone with an average molecular weight of 40,000 in a weight ratio of 4:1;

[0025] The raw materials of the high carbon steel ball blank include, by weight percentage: C 0.9%, Cr 8%, Mo 0.3%, V 0.4%, and the balance is Fe and inevitable impurities.

[0026] Example 2

[0027] A preparation method of a high-hardness steel ball by liquid quenching, comprising the following steps: taking a high-carbon steel ball blank, first heating it to 650°C, keeping it warm for 1 hour, then heating it to 880°C, keeping it warm for 1 hour, then heating it to 1100°C, keeping it warm for 2 hours to perform austenitization treatment, then adding it to a quenching medium at a temperature of 30°C, quenching it until the surface temperature of the high-carbon steel ball is the same as the temperature of the quenching medium, taking it out, tempering it at 210°C in a tempering furnace for 3 hours, taking it out, and air cooling it to room temperature to obtain a high-hardness steel ball;

[0028] Wherein, the quenching medium is an aqueous solution containing 8wt% polyalkylene glycol and 0.8wt% polyvinyl pyrrolidone;

[0029] The average molecular weight of polyalkylene glycol is 25000;

[0030] The polyvinyl pyrrolidone is composed of polyvinyl pyrrolidone with an average molecular weight of 1,400,000 and polyvinyl pyrrolidone with an average molecular weight of 50,000 in a weight ratio of 3:1;

[0031] The raw materials of the high carbon steel ball blank include, by weight percentage: C 1.1%, Cr 6%, Mo 0.35%, V 0.35%, and the balance is Fe and inevitable impurities.

[0032] Example 3

[0033] A preparation method of a high-hardness steel ball by liquid quenching treatment, comprising the following steps: taking a high-carbon steel ball blank, first heating it to 650°C, keeping it warm for 1 hour, then heating it to 880°C, keeping it warm for 1 hour, then heating it to 1000°C, keeping it warm for 2.5 hours to perform austenitization treatment, then adding it to a quenching medium at a temperature of 35°C, quenching it until the surface temperature of the high-carbon steel ball is the same as the temperature of the quenching medium, taking it out, tempering it at 200°C in a tempering furnace for 4 hours, taking it out, and air cooling it to room temperature to obtain a high-hardness steel ball;

[0034] Wherein, the quenching medium is an aqueous solution containing 7wt% polyalkylene glycol and 0.7wt% polyvinyl pyrrolidone;

[0035] The average molecular weight of polyalkylene glycol is 23000;

[0036] The polyvinyl pyrrolidone is composed of polyvinyl pyrrolidone with an average molecular weight of 1,500,000 and polyvinyl pyrrolidone with an average molecular weight of 45,000 in a weight ratio of 3.5:1;

[0037] The raw materials of the high carbon steel ball blank include, by weight percentage: C 1.0%, Cr 7%, Mo 0.3%, V 0.38%, and the balance is Fe and inevitable impurities.

[0038] Comparative Example 1

[0039] The quenching medium is water at a temperature of 35°C, and the rest is the same as in Example 3.

[0040] Comparative Example 2

[0041] The quenching medium does not contain polyvinyl pyrrolidone, and the rest is the same as in Example 3.

[0042] Comparative Example 3

[0043] The quenching medium does not contain polyalkylene glycol, and the rest is the same as in Example 3.

[0044] Comparative Example 4

[0045] In the quenching medium, the polyvinyl pyrrolidone is polyvinyl pyrrolidone with an average molecular weight of 1,500,000, and the rest is the same as in Example 3.

[0046] Comparative Example 5

[0047] In the quenching medium, the polyvinyl pyrrolidone is polyvinyl pyrrolidone with an average molecular weight of 45,000, and the rest is the same as in Example 3.

[0048] Comparative Example 6

[0049] The raw material of the high carbon steel ball blank contains 0.30% V, and the rest is the same as in Example 3.

[0050] Comparative Example 7

[0051] In the raw materials of the high carbon steel ball blank, V is 0.45%, and the rest is the same as in Example 3.

[0052] The steel balls prepared in Examples 1-3 and Comparative Examples 1-7 were tested for their performance, and the number of steel balls with cracks and splits was counted among 100 steel balls produced. The results are shown in Table 1. The diameter of the steel balls was 80 mm.

[0053] Table 1 Test results

[0054]

[0055]

[0056] It can be seen from Table 1 that the steel balls prepared by the method of the present invention have good hardness, the difference between the core and the surface hardness is less than 2HRC, the toughness is good, and the number of steel balls with cracks and cracks is very small.

[0057] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for preparing a high-hardness steel ball by liquid quenching, characterized in that: The method comprises the following steps: taking a high-carbon steel ball blank and subjecting it to austenitization treatment, and then quenching and tempering to obtain a high-hardness steel ball; wherein the quenching medium is an aqueous solution containing polyalkylene glycol and polyvinyl pyrrolidone.

2. The method for preparing a high-hardness steel ball by liquid quenching treatment according to claim 1, characterized in that: In the quenching medium, the mass fraction of polyalkylene glycol is 6-8wt%, and the mass fraction of polyvinyl pyrrolidone is 0.6-0.8wt%.

3. The method for preparing a high-hardness steel ball by liquid quenching treatment according to claim 1 or 2, characterized in that: The average molecular weight of the polyalkylene glycol is 20,000-25,000.

4. The method for preparing a high-hardness steel ball by liquid quenching according to any one of claims 1 to 3, characterized in that: The polyvinyl pyrrolidone is composed of polyvinyl pyrrolidone with an average molecular weight of 1400000-1600000 and polyvinyl pyrrolidone with an average molecular weight of 40000-50000; preferably, the weight ratio of polyvinyl pyrrolidone with an average molecular weight of 1400000-1500000 and polyvinyl pyrrolidone with an average molecular weight of 40000-50000 is 3-4:

1.

5. The method for preparing a high-hardness steel ball by liquid quenching according to any one of claims 1 to 4, characterized in that: The temperature of the quenching medium is 30-40°C.

6. The method for preparing a high-hardness steel ball by liquid quenching according to any one of claims 1 to 5, characterized in that: The raw materials of the high carbon steel ball blank include, by weight percentage: C 0.9-1.1%, Cr 6-8%, Mo0.3-0.35%, V 0.35-0.4%, and the balance is Fe and inevitable impurities.

7. The method for preparing a high-hardness steel ball by liquid quenching according to any one of claims 1 to 6, characterized in that: The raw materials of the high carbon steel ball blank include, by weight percentage: C 1.0%, Cr 7%, Mo 0.3%, V 0.38%, and the balance is Fe and inevitable impurities.

8. The method for preparing a high-hardness steel ball by liquid quenching according to any one of claims 1 to 7, characterized in that: The austenitizing temperature is 990-1100°C and the time is 2-3h.

9. The method for preparing a high-hardness steel ball by liquid quenching according to any one of claims 1 to 8, characterized in that: The tempering temperature is 190-210℃ and the tempering time is 3-5h.

10. The method for preparing a high-hardness steel ball by liquid quenching according to any one of claims 1 to 9, characterized in that: After tempering, air cool to room temperature.