Method for recovering cobalt from waste liquid leached from waste lithium cobalt oxide positive electrode material through organic system
By using organic systems to leaching and separation of cobalt ions in waste lithium batteries, the complexity of separation steps between cobalt lithium and aluminum foil and environmental pollution problems are solved, efficient and low-cost cobalt recycling is achieved, and the extraction of cobalt ions is significantly improved. Rate.
Patent Information
- Application Number
- CN202410588686.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-13
- Publication Date
- 2024-11-08
AI Technical Summary
The prior art is complex in recycling cobalt ions in waste lithium cobalt oxide batteries, with high cost and environmental pollution risks, especially the separation steps between cobalt lithium and aluminum foil are difficult to simplify.
Using an organic system, the positive electrode material of the used lithium battery is mechanically crushed in saturated brine, and then soaked with ethanol/ethylene glycol mixed solution and organic polycarboxylic acid. The cobalt ions and lithium ions are leached through heating and stirring, and the cobalt ions are leached in horses. Calcination and precipitation in the furnace to obtain high-purity cobalt tetraoxide particles, avoiding the use of strong alkalis and strong acids.
The separation steps between cobalt lithium and aluminum foil are significantly simplified, the emission of industrial waste liquid is reduced, the cost of cobalt recovery in lithium cobalt oxide is reduced, and the extraction rate of cobalt ions is increased, and equipment corrosion and environmental pollution are reduced.
Smart Images

Figure CN118910408A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for recovering cobalt from waste lithium ion batteries, in particular to a method for recovering cobalt from waste cobalt oxide positive electrode material leaching waste liquid using an organic system, and belongs to the field of resource utilization of lithium ion battery waste. Background Art
[0002] With the rapid development of new energy fields such as electric vehicles and energy storage batteries, the demand for lithium cobalt oxide batteries, as a core component, has been rising year by year. However, the treatment and recycling of waste lithium cobalt oxide batteries has gradually become prominent. Lithium cobalt oxide batteries have attracted attention due to their stable structure, high specific capacity and excellent performance, and are widely used in electronic products such as notebooks and mobile phones. Its positive electrode contains cobalt and lithium, which are scarce resources, so their recycling value is significant. However, the lithium cobalt oxide positive electrode sheet is densely made, and conventional crushing methods make it difficult to separate the lithium cobalt oxide powder from the aluminum foil. It is usually necessary to use a strong alkali to dissolve the aluminum foil first, and then perform subsequent treatment on the lithium cobalt oxide. This process is more complicated, the cost is higher, and the strong alkaline solution is also prone to environmental pollution.
[0003] In the subsequent treatment of lithium cobalt oxide, it is usually necessary to use inorganic strong acids, complexes such as sodium thiosulfate, hydrogen peroxide and other reducing agents to leach cobalt and lithium from the positive electrode material, and then use alkali to neutralize the excess hydrogen ions in the leachate. After the pH of the leachate is adjusted to near neutral, sodium carbonate and other precipitants are used to precipitate the cobalt ions and lithium ions step by step. Although these processes have advantages such as high yield, they also have disadvantages such as complex processes and high costs. In addition, the large-scale use of inorganic strong acids and alkalis also has the potential to corrode equipment and pose a greater risk of environmental pollution.
[0004] In this context, developing a new process that is simple, has little corrosion to equipment, and is environmentally friendly to recycle cobalt ions from waste lithium-ion batteries will have significant social effects. Summary of the invention
[0005] The technical problem to be solved by the present invention is to overcome the above-mentioned shortcomings and provide a method for recovering cobalt from waste liquor leached from waste lithium cobalt oxide positive electrode materials using an organic system.
[0006] To achieve the above objectives, the method of the present application includes:
[0007] (1) The waste lithium battery is immersed in saturated salt water and fully discharged, and then mechanically crushed and separated to separate the positive electrode material, negative electrode material, separator, etc. in the battery, and obtain the positive electrode material.
[0008] (2) Crushing the positive electrode material: Crushing the positive electrode material containing aluminum foil into small pieces of 20 mm to 30 mm square.
[0009] (3) The crushed positive material is uniformly mixed and soaked in an ethanol / ethylene glycol mixed solution to form a soaking solution A, wherein the molar ratio of ethanol to ethylene glycol is between 1:10 and 10:1.
[0010] Preferably, 5 to 10 ml of organic solvent is used to soak each gram of lithium cobalt oxide positive electrode sheet.
[0011] (4) A certain amount of organic polycarboxylic acid is added to the mixed solvent to form solution B.
[0012] Preferably, 1 gram of organic acid is used per gram of lithium cobalt oxide positive electrode sheet.
[0013] (5) The solution is heated and maintained for a certain period of time under stirring conditions to obtain a leachate C. At this time, most of the cobalt ions and lithium ions are leached into the solvent by the organic acid. Since the organic acid is weak in acidity, the aluminum foil remains basically intact. At the same time, since ethylene glycol has reducing properties, no additional reducing agent does not need to be added in this step of the reaction.
[0014] Preferably, the temperature range is between 80°C and 160°C, and maintained for 1-2 hours;
[0015] Preferably, the stirring speed is 500-700 r / min.
[0016] (6) Cooling the leaching solution C and filtering it to separate the insoluble matter in the leaching solution C, thereby obtaining the leaching solution D, and separating the cobalt and lithium in the aluminum foil and the positive electrode material.
[0017] (7) The leaching solution D is heated again under stirring conditions and maintained for a certain period of time, and the cobalt ions in the leaching solution D are precipitated in the form of a complex.
[0018] Preferably, the stirring speed is 500-700 r / min.
[0019] Preferably, the heating temperature is 80-160° C. and the heating time is 2-4 hours.
[0020] (8) The precipitate is calcined in a muffle furnace to remove the organic ligands and obtain cobalt tetroxide particles with higher purity.
[0021] Preferably, the muffle furnace calcination temperature is 500-600° C., and the calcination time is 1-2 hours.
[0022] Compared with the prior art, the beneficial effects of this application include:
[0023] The present invention provides a method for recovering cobalt from waste cobalt oxide lithium positive electrode material leaching waste liquid by an organic system, which realizes the selective leaching of cobalt and lithium in the cobalt oxide lithium positive electrode material, and significantly simplifies the separation step of cobalt, lithium and aluminum foil. The method realizes the direct precipitation separation of cobalt ions in the leachate, avoids the steps of adjusting the pH value with alkali, adding a reducing agent, adding a precipitating agent, etc., greatly simplifies the reaction steps, reduces the discharge of industrial waste liquid, and can ultimately significantly reduce the cost of recovering cobalt in cobalt oxide lithium. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 The figure is a schematic flow chart of the method for recycling lithium cobalt oxide positive electrode sheets of the present invention. DETAILED DESCRIPTION
[0025] The technical scheme of the present invention is further described in detail below in conjunction with the embodiments, but they are not intended to limit the present invention.
[0026] In the following examples, the leaching rate is calculated by measuring the ratio of the mass of cobalt in the leaching solution to the mass of the positive electrode active material. The calculation formula for the leaching rate (R) of the metal is:
[0027]
[0028] Wherein: R—metal leaching efficiency (%); c—metal concentration of leachate (g / L); V—leachate volume (L); n—leachate dilution factor; m—weighed mass of lithium cobalt oxide sample (g); w—mass proportion of valuable metals (%).
[0029] Example 1
[0030] The waste lithium battery was immersed in saturated salt water and fully discharged, then mechanically crushed and separated. 50g of the positive electrode material with aluminum foil was mixed with 100mL of ethylene glycol / ethanol mixed solution (molar ratio of 3:1), 40g of malic acid was added and the solution was heated to 140°C for 1 hour under stirring conditions. The resulting mixed solution was cooled to room temperature and filtered, and the resulting filtrate was purple-red. The filtrate was then heated and stirred again to 140°C and continued to be heated for 3 hours to obtain a large amount of purple-red precipitate. The precipitate was filtered and dried and calcined in a muffle furnace at 500°C for 1 hour to obtain a black cobalt tetroxide powder with high purity.
[0031] According to the above leaching rate (R) calculation formula, the cobalt extraction rate in the leaching solution is 97.5%, which proves that the cobalt recovery method of lithium cobalt oxide positive electrode sheet in Example 1 has a good effect in recovering cobalt.
[0032] Example 2
[0033] Immerse the waste lithium battery in saturated salt water, fully discharge it, and then mechanically crush and separate it to separate the positive electrode material with aluminum foil. Take 100g of the positive electrode material with aluminum foil and mix it with 200mL of ethylene glycol / ethanol mixed solution (molar ratio of 3:1), add 80g of malic acid and heat the solution to 140℃ for 1 hour under stirring conditions, cool the resulting mixed solution to room temperature and filter it, and the resulting filtrate is purple-red. Then heat the filtrate again with stirring and heat it to 140℃ and continue heating for 3 hours to obtain a large amount of purple-red precipitate. Filter and dry the precipitate and calcine it in a muffle furnace at 500℃ for 1 hour to obtain a black cobalt tetroxide powder with high purity.
[0034] According to the above leaching rate (R) calculation formula, the cobalt extraction rate in the leaching solution is 99.4%, which proves that the cobalt recovery method of lithium cobalt oxide positive electrode sheet in Example 2 has a good effect in recovering cobalt.
[0035] Example 3
[0036] Immerse the waste lithium battery in saturated salt water, fully discharge it, and then mechanically crush and separate it to separate the positive electrode material with aluminum foil. Take 150g of the positive electrode material with aluminum foil and mix it with 200mL of ethylene glycol / ethanol mixed solution (molar ratio of 3:1), add 80g of malic acid and heat the solution to 140℃ for 1 hour under stirring conditions, cool the resulting mixed solution to room temperature and filter it, and the resulting filtrate is purple-red. Then heat the filtrate again with stirring and heat it to 140℃ and continue heating for 3 hours to obtain a large amount of purple-red precipitate. Filter and dry the precipitate and calcine it in a muffle furnace at 500℃ for 1 hour to obtain a black cobalt tetroxide powder with high purity.
[0037] According to the above leaching rate (R) calculation formula, the cobalt extraction rate in the leaching solution is 97.6%, which proves that the cobalt oxide positive plate recovery method of Example 3 has a good effect in recovering cobalt.
[0038] Example 4
[0039] Immerse the waste lithium battery in saturated salt water, fully discharge it, and then mechanically crush and separate it to separate the positive electrode material with aluminum foil. Take 200g of the positive electrode material with aluminum foil and mix it with 200mL of ethylene glycol / ethanol mixed solution (molar ratio of 3:1), add 80g of malic acid and heat the solution to 140℃ for 1 hour under stirring conditions, cool the resulting mixed solution to room temperature and filter it, and the resulting filtrate is purple-red. Then heat the filtrate again with stirring and heat it to 140℃ and continue heating for 3 hours to obtain a large amount of purple-red precipitate. Filter and dry the precipitate and calcine it in a muffle furnace at 500℃ for 1 hour to obtain a black cobalt tetroxide powder with high purity.
[0040] The cobalt extraction rate in the leaching solution calculated according to the above leaching rate (R) calculation formula is 84.4%. It is proved that Example 4 increases the content of the lithium cobalt oxide positive electrode sheet, and the recovery needs to increase the concentration of the malic acid and ethylene glycol / ethanol mixed solution to promote the leaching process.
[0041] The specific embodiments of the present invention have been described in detail above, but the present invention is not limited to the above embodiments.
Claims
1. A method for recovering cobalt from waste cobalt oxide lithium positive electrode material leaching waste liquid by an organic system, characterized in that: The following steps are involved: (1) The recycled waste lithium battery is placed in a saturated NaCl solution and fully discharged; (2) obtaining positive electrode materials by mechanical crushing and separation; (3) soaking the positive electrode material in an organic solvent to form a soaking solution A; (4) adding a certain amount of organic acid to the soaking solution to form solution B, heating solution B under stirring conditions and maintaining the temperature for a certain period of time to obtain an extract solution C; (5) filtering the extract C for the first time to separate the insoluble matter in the extract C to obtain the extract D; (6) The leaching solution D is heated again under stirring conditions and maintained for a certain period of time, and the cobalt ions in the leaching solution D are precipitated in the form of a complex; (7) Collecting the precipitate, calcining the precipitate in a muffle furnace to remove the organic ligand and obtain cobalt tetroxide solid.
2. The recycling method according to claim 1, characterized in that: The organic acid in step (4) includes polybasic organic carboxylic acid.
3. The recycling method according to claim 2, characterized in that: The polybasic organic carboxylic acid includes any one or more of malic acid, citric acid, oxaloacetic acid and tartaric acid.
4. The recycling method according to claim 2, characterized in that: The organic solvent in step (3) comprises a mixed solvent of ethanol and ethylene glycol, and the molar ratio of the mixed solvent is 1:10-10:
1.
5. The recycling method according to claim 1, characterized in that: The amount of organic solvent used in step (3) is 5 to 10 ml of organic solvent per gram of lithium cobalt oxide positive electrode sheet.
6. The recycling method according to claim 1, characterized in that: The amount of organic acid added in step (4) is 1 gram of organic acid per gram of lithium cobalt oxide positive electrode sheet.
7. The recycling method according to claim 1, characterized in that: The heating temperature in step (4) is 80° C. to 160° C., and the holding time is 1 to 2 hours.
8. The recycling method according to claim 1, characterized in that: The heating temperature in step (6) is 80° C. to 160° C., and the holding time is 2 to 4 hours.
9. The recycling method according to claim 1, characterized in that: The holding time in step (6) is 2 to 6 hours.
10. The recycling method according to claim 1, characterized in that: The calcination temperature in step (7) is 500° C. and the calcination time is 1 to 2 hours.