Method for efficiently separating rhenium and arsenic from copper smelting rhenium-rich slag
By using sodium thiosulfate precipitation method and selective chlorination method in copper smelting waste acid, combined with low-temperature volatilization process, the efficient separation of rhenium and arsenic is solved, the recovery rate of rhenium and product quality are improved, and environmental pollution is reduced and energy consumption, achieving efficient and low-cost separation effect of rhenium and arsenic.
Patent Information
- Application Number
- CN202410959469.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-08
AI Technical Summary
The prior art is difficult to efficiently remove arsenic when extracting rhenium from copper smelting waste acid, resulting in a large amount of harmful arsenic in rhenium-rich slag, which affects product quality. In addition, the traditional pyrometallurgy roasting and hydrometallurgy arsenic removal process has high energy consumption. , problems of low environmental pollution and recovery rates.
After the chemical precipitation method of sodium thiosulfate, the pH value of copper smelting waste acid is adjusted through selective chlorination and low-temperature volatility processes, and react with hydrochloric acid under low temperature and heating conditions to separate the rhenium-rich slag with high rhenium content. Reduce the residue of arsenic, reduce the ignition temperature and reduce the amount of waste liquid.
It has achieved efficient removal of arsenic from rhenium-rich slag without losing rhenium, improve rhenium grade, reduce operating environment risks, reduce environmental pollution, and improve rhenium recovery and separation effect without losing rhenium. The process is short and the cost is low.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of recycling and utilizing secondary resources of rare and precious metals, and in particular to a method for efficiently separating rhenium and arsenic from rhenium-rich slag from copper smelting. Background Art
[0002] Rhenium is one of the rarest elements in the Earth's crust, with an average abundance of about 1 ppb (10 - 9 ). There is almost no independent mineralization in nature, and it is mostly associated with molybdenite and bornite. It is mainly used in modern high-tech fields such as national defense, aerospace, nuclear energy and electronic industry. The growing demand and relatively scarce reserves have led to a serious imbalance between the supply and demand of rhenium. Therefore, it is urgent to improve the recovery rate of rhenium and expand the channels for obtaining rhenium. Since rhenium has no independent deposits in nature, rhenium resources mostly come from smelting waste slag and rhenium-containing secondary resources, such as molybdenum concentrate roasting flue gas leaching liquid, copper waste acid and high-temperature alloys. Among them, copper waste acid is an important rhenium-containing resource, which is produced in the acid-making process of copper pyrometallurgy. During the high-temperature smelting process of copper concentrate, since the boiling point of Re2O7 is 361°C and it has high volatility, Re2O7 will eventually enter the flue in the form of flue gas. The flue gas entering the flue will eventually form flue ash in the form of Re2O7 solid particles due to the decrease in temperature. After dust collection, rhenium enters the acid production system along with sulfur dioxide. After leaching and purification, the rhenium-containing flue gas is enriched in the washing waste acid, that is, the copper smelting waste acid, in the form of perrhenate ions.
[0003] The current methods for extracting rhenium from waste acid from copper smelting mainly include chemical precipitation, solvent extraction, ion exchange and adsorption. In the solvent extraction method, a large amount of solvent will be consumed during the extraction process, and the evaporation amount will also increase, causing environmental pollution and deteriorating the production environment. At the same time, attention should be paid to the hazards of the organic extractant itself and the environmental hazards of its interaction with strong oxidants. In the ion exchange method, a large amount of wastewater will be generated during its separation process, and direct discharge will cause great harm to the environment. The cost of wastewater purification is not low, and additional energy consumption is increased. The biggest drawback of the adsorption method is that the adsorption mechanism is too simple, lacks recognition and intelligence, and it is difficult to show satisfactory selective adsorption for a variety of substances with similar spatial structures and properties. Compared with the above methods, the sodium thiosulfate chemical precipitation method has stronger selectivity for rhenium precipitation and higher rhenium precipitation rate, which ultimately leads to a higher rhenium content in the rhenium-rich slag in the precipitate (about 1%~10%), and sodium thiosulfate has strong adaptability to waste acids with various rhenium concentrations. Therefore, the use of sodium thiosulfate for precipitation has great prospects for the enrichment of rhenium in waste acid. However, it is worth noting that the rhenium-rich slag obtained by the sodium thiosulfate chemical precipitation method contains a large amount of arsenic, which is extremely dangerous because it enters the leachate in the form of ions and ultimately reduces the quality of the product.
[0004] At present, the treatment methods of arsenic-containing waste slag are mainly pyrometallurgical roasting and hydrometallurgical leaching. Among them, the principle of arsenic removal by pyrometallurgical roasting is to use the difference in volatility between arsenic and other precious metal compounds to volatilize and separate arsenic trioxide under high temperature conditions. Pyrometallurgical roasting has the disadvantages of small range of raw materials suitable for processing, large capital investment, poor working environment, and low recovery rate. The principle of hydrometallurgical arsenic removal is that arsenic or other elements in dust are dissolved by reaction with leaching agent, arsenic is transferred from solid phase to liquid phase, and removed in liquid phase, finally achieving the purpose of separating arsenic from valuable metals. The main disadvantages of hydrometallurgical leaching are large amount of waste liquid, high equipment requirements, unstable products, and low recovery rate. Therefore, whether it is pyrometallurgical roasting or hydrometallurgical leaching, there are some technical problems that need to be improved, which limits the application of these processes in industrial production. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a simple and efficient method for separating rhenium and arsenic from rhenium-rich slag in copper smelting.
[0006] In order to solve the above problems, the present invention discloses a method for efficiently separating rhenium and arsenic from rhenium-rich slag from copper smelting, which is characterized in that: the method uses copper smelting waste acid as raw material, first adjusts its pH with alkali, then adds sodium thiosulfate to react, and filters after the reaction, and the obtained precipitate is rhenium-rich slag A; the rhenium-rich slag A is ground and sieved, and then a hydrochloric acid solution with a concentration of 6.00 mol / L to 12.00 mol / L is added, stirred evenly, first reacted at low temperature and then reacted and separated under heating conditions, and the obtained precipitate after the reaction is washed and dried to obtain rhenium-rich slag B.
[0007] The rhenium concentration in the copper smelting waste acid is 0.01-0.05 g / L, and the arsenic concentration is 1-5 g / L.
[0008] The alkali refers to a sodium hydroxide solution with a concentration of 1-4 mol / L, and the pH is adjusted to 1-3.
[0009] Based on 1 L of copper smelting waste acid, the added amount of sodium thiosulfate is 15g~20g.
[0010] The reaction conditions are a temperature of 40°C to 50°C and a time of 100 min to 120 min.
[0011] The rhenium-rich slag A is ground and passed through a 100-200 mesh sieve.
[0012] The solid-liquid mass ratio of the rhenium-rich slag A to the hydrochloric acid solution is 1:10-1:15.
[0013] The low temperature reaction conditions refer to a temperature of 60°C to 80°C and a time of 40min to 60min.
[0014] The heating conditions are as follows: the temperature is 200°C to 300°C and the time is 60min to 100min.
[0015] The washing and drying conditions refer to washing with ultrapure water for 2 to 3 times and drying at 45° C. for 12 hours.
[0016] Compared with the prior art, the present invention has the following advantages: 1. The present invention innovatively proposes a process of selective chlorination and low-temperature volatilization for As2S3, As2O3, ReS2 and ReO2 contained in the rhenium-rich slag obtained by the sodium thiosulfate chemical precipitation method using copper smelting waste acid, so as to remove the harmful element arsenic in the rhenium-rich slag without almost losing the rhenium element, thereby further improving the rhenium grade in the rhenium-rich slag.
[0017] 2. The present invention adopts selective chlorination and low-temperature volatilization process, which can not only reduce the temperature in the pyrometallurgical roasting process, but also solve the problem of large amount of waste liquid in the hydrometallurgical leaching process, avoiding secondary environmental pollution.
[0018] 3. The present invention directly chlorinates arsenide into low-toxic arsenic chloride instead of highly toxic arsenic oxide through the chlorination method, thereby reducing the risk of the operating environment to a certain extent.
[0019] 4. Compared with the traditional hydrometallurgical and pyrometallurgical separation technologies of rhenium and arsenic in rhenium-rich slag, the method of the present invention has good rhenium and arsenic separation effect, high rhenium recovery rate and low energy consumption.
[0020] 4. The present invention has short process, low cost and easy operation. DETAILED DESCRIPTION
[0021] A method for efficiently separating rhenium and arsenic from rhenium-rich slag from copper smelting: the method is to use copper smelting waste acid with a rhenium concentration of 0.01-0.05 g / L and an arsenic concentration of 1-5 g / L as raw materials, first adjust its pH to 1-3 with a sodium hydroxide solution with a concentration of 1-4 mol / L, and then add 15g-20g of sodium thiosulfate per 1 L of copper smelting waste acid for reaction at a temperature of 40°C-50°C and a time of 100min-120min. After the reaction is completed, the precipitate is filtered, and the obtained precipitate is rhenium-rich slag A. After the rhenium-rich slag A is ground through a 100-mesh sieve to a 200-mesh sieve, a hydrochloric acid solution with a concentration of 6.00 mol / L-12.00 mol / L is added, and the solid-liquid mass ratio (g / g) of the rhenium-rich slag A to the hydrochloric acid solution is 1:10-1:15. Stir evenly, first react at a low temperature of 60℃~80℃ for 40min~60min, then heat at 200℃~300℃ for reaction and separation for 60min~100min. After the reaction, the precipitate obtained is washed with ultrapure water 2~3 times and dried at 45℃ for 12h to obtain rhenium-rich slag B.
[0022] Example 1 A method for efficiently separating rhenium and arsenic from rhenium-rich slag from copper smelting: the method comprises taking 200 mL of copper smelting waste acid containing a rhenium concentration of 0.025 g / L and an arsenic concentration of 2.9 g / L as a raw material, first adjusting the pH value of the copper smelting waste acid to 2 with a sodium hydroxide solution having a concentration of 4 mol / L, then adding 15 g / L of sodium thiosulfate, reacting at 40°C for 120 min, filtering after the reaction, and obtaining the precipitate as rhenium-rich slag A. Rhenium-rich slag A was ground and sieved with 100 mesh. 0.15 g of rhenium-rich slag A (rhenium content was 1.103%, arsenic content was 14.3%) was weighed, 1.5 g of 6 mol / L hydrochloric acid solution was added to the rhenium-rich slag A and stirred evenly. The mixture was reacted at 60°C-80°C for 40 min, and then reacted and separated at 200°C for 100 min. After the reaction, the precipitate was washed with ultrapure water for 2-3 times and dried at 45°C for 12 h to obtain 0.0345 g of rhenium-rich slag B (rhenium content was 4.79%, arsenic content was 0.84%).
[0023] After characterization, the rhenium content in the final rhenium-rich slag B product is 4.79%, the comprehensive recovery rate of rhenium is as high as 98.97%, the volatilization rate of arsenic is as high as 98.65%, and the rhenium-arsenic separation effect is good.
[0024] Example 2 A method for efficiently separating rhenium and arsenic from rhenium-rich slag from copper smelting: the method comprises taking 200 mL of copper smelting waste acid containing a rhenium concentration of 0.025 g / L and an arsenic concentration of 2.9 g / L as a raw material, first adjusting the pH value of the copper smelting waste acid to 1 with a sodium hydroxide solution having a concentration of 4 mol / L, then adding 20 g / L of sodium thiosulfate, reacting at 45°C for 110 min, filtering after the reaction, and obtaining the precipitate as rhenium-rich slag A. Rhenium-rich slag A was ground and sieved through 150 mesh. 1.5 g of rhenium-rich slag A (rhenium content was 1.103%, arsenic content was 15.6%) was weighed, 22.5 g of 12 mol / L hydrochloric acid solution was added to the rhenium-rich slag A and stirred evenly. The mixture was reacted at 60°C-80°C for 50 min, and then reacted and separated at 250°C for 1 h. After the reaction, the precipitate was washed with ultrapure water for 2-3 times and dried at 45°C for 12 h to obtain 0.3361 g of rhenium-rich slag B (rhenium content was 4.92%, arsenic content was 1.01%).
[0025] After characterization, the rhenium content in the final rhenium-rich slag B product is 4.92%, the comprehensive recovery rate of rhenium is as high as 98.80%, the volatilization rate of arsenic is as high as 98.55%, and the rhenium-arsenic separation effect is good.
[0026] Example 3 A method for efficiently separating rhenium and arsenic from rhenium-rich slag from copper smelting: the method comprises taking 200 mL of copper smelting waste acid containing 0.025 g / L rhenium and 2.9 g / L arsenic as raw materials, first adjusting the pH value of the copper smelting waste acid to 3 with a 4 mol / L sodium hydroxide solution, then adding 17.5 g / L sodium thiosulfate, reacting at 50°C for 100 min, filtering after the reaction, and obtaining the precipitate as rhenium-rich slag A. Rhenium-rich slag A was ground and sieved with 200 mesh. 1.0 g of rhenium-rich slag A (rhenium content was 1.103%, arsenic content was 14.9%) was weighed, 12.5 g of 9 mol / L hydrochloric acid solution was added to the rhenium-rich slag A and stirred evenly. The mixture was reacted at 60°C-80°C for 60 min, and then reacted and separated at 225°C for 80 min. After the reaction, the precipitate was washed with ultrapure water for 2-3 times and dried at 45°C for 12 h to obtain 0.2301 g of rhenium-rich slag B (rhenium content was 4.78%, arsenic content was 0.906%).
[0027] After characterization, the rhenium content in the final rhenium-rich slag B product is 4.78%, the comprehensive recovery rate of rhenium is as high as 98.86%, the volatilization rate of arsenic is as high as 98.60%, and the rhenium-arsenic separation effect is good.
[0028] The above examples are only specific examples for clearly illustrating the present invention, and do not constitute a limitation of the present invention. For the experimenters of the present invention, the contents can be modified and supplemented within the scope of the claims of the present invention as required. All changes proposed in the technical scheme and technical ideas of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for efficiently separating rhenium and arsenic from rhenium-rich slag from copper smelting, characterized in that: The method is to use copper smelting waste acid as a raw material, first adjust the pH thereof with alkali, then add sodium thiosulfate to react, filter after the reaction is completed, and the obtained precipitate is rhenium-rich slag A; the rhenium-rich slag A is ground and sieved, and then a hydrochloric acid solution with a concentration of 6.00 mol / L to 12.00 mol / L is added, stirred evenly, first reacted at a low temperature and then reacted and separated under heating conditions, and after the reaction is completed, the obtained precipitate is washed and dried to obtain rhenium-rich slag B.
2. A method for efficiently separating rhenium and arsenic from rhenium-rich slag from copper smelting as claimed in claim 1, characterized in that: The rhenium concentration in the copper smelting waste acid is 0.01-0.05 g / L, and the arsenic concentration is 1-5 g / L.
3. A method for efficiently separating rhenium and arsenic from rhenium-rich slag from copper smelting as claimed in claim 1, characterized in that: The alkali refers to a sodium hydroxide solution with a concentration of 1-4 mol / L, and the pH is adjusted to 1-3.
4. A method for efficiently separating rhenium and arsenic from rhenium-rich slag from copper smelting as claimed in claim 1, characterized in that: Based on 1L of copper smelting waste acid, the added amount of sodium thiosulfate is 15g~20g.
5. A method for efficiently separating rhenium and arsenic from rhenium-rich slag from copper smelting as claimed in claim 1, characterized in that: The reaction conditions are a temperature of 40°C to 50°C and a time of 100 min to 120 min.
6. A method for efficiently separating rhenium and arsenic from rhenium-rich slag from copper smelting as claimed in claim 1, characterized in that: The rhenium-rich slag A is ground and passed through a 100-200 mesh sieve.
7. A method for efficiently separating rhenium and arsenic from rhenium-rich slag from copper smelting as claimed in claim 1, characterized in that: The solid-liquid mass ratio of the rhenium-rich slag A to the hydrochloric acid solution is 1:10-1:
15.
8. A method for efficiently separating rhenium and arsenic from rhenium-rich slag from copper smelting as claimed in claim 1, characterized in that: The low temperature reaction conditions refer to a temperature of 60°C to 80°C and a time of 40min to 60min.
9. A method for efficiently separating rhenium and arsenic from rhenium-rich slag from copper smelting as claimed in claim 1, characterized in that: The heating conditions are as follows: the temperature is 200°C to 300°C and the time is 60min to 100min.
10. A method for efficiently separating rhenium and arsenic from rhenium-rich slag from copper smelting as claimed in claim 1, characterized in that: The washing and drying conditions refer to washing with ultrapure water for 2 to 3 times and drying at 45° C. for 12 hours.
Citation Information
Cited By
Method for recovering rhenium concentrate from flue gas leacheate generated in molybdenum concentrate roasting process
CN121538478A