Method for preparing ultrathin high-thermal-conductivity copper-diamond composite material through tape casting
Ultra-thin, high thermal conductivity copper diamond composite materials are prepared through casting forming process, which solves the problems of large thickness and non-processability of copper diamond composite materials in the prior art, and realizes high thermal conductivity and low cost copper diamond composite materials, which are suitable for miniaturization Electronics.
Patent Information
- Application Number
- CN202410954298.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-08
AI Technical Summary
It is difficult to prepare ultra-thin copper diamond composite materials in the prior art, and the copper diamond composite materials are thicker in thickness, poor surface machiningability, and high production cost, making it difficult to meet the heat dissipation needs of high-performance and miniaturized electronic devices.
Using casting molding technology, diamond particles are processed by boron plating to prepare copper alloy casting blanks and metal copper mesh skeletons to form an ultra-thin, high thermal conductivity copper diamond composite material with sandwich structure, and uses B, Ti, and Cr in copper alloy powder. , Zr elements reduce the melting point of copper, improve thermal conductivity, and enhance the density of the material through high temperature pressure sintering.
It has achieved copper diamond composite materials with high thermal conductivity (>480W/mK), ultra-thin thickness (0.2~0.4mm), light density and good surface processability. It is suitable for miniaturized electronic components, with low process cost and suitable for industry .
Smart Images

Figure CN118910449A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of layered products composed of copper, and in particular relates to a method for preparing an ultra-thin high thermal conductivity copper-diamond composite material by tape casting. Background Art
[0002] As the demand for new electronic devices continues to increase, electronic devices are developing towards high performance, miniaturization and high integration. Traditional heat dissipation materials have gradually become unable to meet the demand for high heat dissipation. Heat dissipation has become one of the technical bottlenecks restricting the development of the electronic information industry. In order to obtain stable performance of electronic devices, heat dissipation conditions must be improved. Therefore, research and development of high-performance packaging materials and heat dissipation materials has become a key link in the development of the electronics industry.
[0003] As a new generation of thermal management materials, copper diamond composite materials have high thermal conductivity and suitable thermal expansion coefficient. In practical application scenarios, the thickness of the composite material needs to be very thin, and before processing or welding the copper diamond composite material, a copper coating is often required on the surface to increase processability and plating. Due to the large difference in electrode potential between diamond and copper, the copper coating prepared by the existing electroplating copper coating method has poor density and is uneven. Therefore, a new preparation method needs to be found to meet the use requirements of copper diamond composite materials.
[0004] CN112974809A provides a method for copper coating on the surface of a diamond / copper composite material, wherein copper foil or copper powder is sintered by SPS sintering until it is melt-infiltrated on the surface of the diamond / copper composite material. The surface has good machinability and plating properties, but the thickness of the diamond / copper composite material is more than 1 mm, and the thickness of the copper coating on the upper and lower surfaces of the diamond / copper composite material is more than 0.1 mm, and the total thickness is too high.
[0005] At present, the main method for preparing copper-diamond composite materials is melt infiltration, in which molten metal copper is infiltrated into the gaps of diamond particle accumulation under the action of protective gas pressure, mechanical extrusion force or capillary force. The size and thickness of the copper-diamond composite material prepared by this method are restricted by the mold. The thickness of the copper-diamond composite material is greater than 0.8mm, and it is difficult to reach less than 0.4mm. Summary of the invention
[0006] The technical problem to be solved by the present invention is to provide a method for preparing an ultra-thin high thermal conductivity copper-diamond composite material by tape casting in view of the above-mentioned deficiencies in the prior art, which solves the problems of thick thickness and unprocessability of the copper-diamond composite material in the prior art, and has controllable preparation cost and high yield rate, and is suitable for industrial application.
[0007] In order to solve the above technical problems, the technical solution provided by the present invention is:
[0008] A method for preparing an ultra-thin high thermal conductivity copper-diamond composite material by tape casting is provided, and the specific steps are as follows:
[0009] 1) boron-plating the surface of diamond particles: diamond particles, boron powder, boric acid powder and magnesium powder are uniformly stirred to obtain a mixed powder, which is laid in an alumina ceramic crucible, and then the alumina ceramic crucible is placed in a high-temperature tube furnace for heat treatment, and after cooling, the crucible is taken out and cleaned to obtain boron-plated diamond particles;
[0010] 2) preparing copper alloy tape casting blank: copper alloy powder, dispersant, binder, plasticizer and organic solvent are ball-milled for 4-8 hours, the slurry obtained by ball milling is defoamed and filtered to obtain copper alloy tape casting slurry, and the obtained copper alloy tape casting slurry is injected into a tape casting machine for tape casting to obtain copper alloy blank;
[0011] 3) preparing a metal copper mesh skeleton: using a copper foil with a thickness of 0.05 to 0.3 mm to be wet-etched to obtain a metal copper mesh skeleton with regularly arranged circular through holes;
[0012] 4) Preparing an ultra-thin high thermal conductivity copper-diamond composite material: cutting the copper alloy blank prepared in step 2) and the metal copper mesh skeleton prepared in step 3) into the same size, then using a layer of copper alloy blank as the bottom layer, then covering a layer of metal copper mesh skeleton and laying the boron-coated diamond particles obtained in step 1) inside the metal copper mesh skeleton, ensuring that each mesh of the metal copper mesh skeleton is filled with boron-coated diamond particles, and finally covering the upper surface of the metal copper mesh skeleton with a layer of copper alloy blank, pressing the stacked sample into shape, and then removing binder, sintering, and polishing to obtain an ultra-thin high thermal conductivity copper-diamond composite material.
[0013] According to the above scheme, in step 1), the particle size of the diamond particles is 100-300 μm; the particle size of the boron powder is 1-5 μm; the particle size of the boric acid powder is 20-30 μm; and the particle size of the magnesium powder is 10-20 μm.
[0014] According to the above scheme, the mass percentage of each component in the mixed powder in step 1) is as follows: 40-45% diamond particles, 10-20% boron powder, 30-40% boric acid powder, and 2-5% magnesium powder.
[0015] According to the above scheme, the heat treatment process conditions in step 1) are: heating to 1100-1500°C at a heating rate of 3-15°C / min at room temperature and keeping warm for 30-60 minutes.
[0016] According to the above scheme, the boron coating thickness on the surface of the boron-coated diamond particles in step 1) is 800 to 1200 nm.
[0017] According to the above scheme, the copper alloy powder in step 2) is vacuum atomized powder, with a particle size of 3-10 μm, and the composition and mass percentage are: B 0.50-1.20%, Ti 0.15-0.55%, Cr 0.50-0.80%, Zr 0.25-0.45%, and the balance is Cu. The copper alloy powder contains elements such as Cr, B, and Zr, which can reduce the melting point of copper during sintering, and accelerate the diffusion of elements to tightly combine copper and diamond, thereby improving thermal conductivity.
[0018] According to the above scheme, the dispersant in step 2) is a mixture of one or more of glyceryl tristearate, phosphate or triethanolamine, the binder is a mixture of one or more of phenolic resin, ethyl cellulose, polyvinyl alcohol or polyvinyl butyral, the plasticizer is a mixture of one or more of glycerol, dioctyl phthalate, polyethylene glycol or propylene glycol, and the organic solvent is a mixture of one or more of butanone, trichloroethylene, isopropyl alcohol or ethyl lactate.
[0019] According to the above scheme, the mass percentages of the copper alloy powder, dispersant, binder, plasticizer and organic solvent in step 2) are as follows: 60-70% copper alloy powder, 1-3% dispersant, 2-5% binder, 2-4% plasticizer and 20-35% organic solvent.
[0020] According to the above scheme, the casting process conditions in step 2) are: the height of the scraper is 0.1-0.3 mm, the casting speed is 60-90 cm / min, and the drying method is shade drying.
[0021] According to the above scheme, the thickness of the copper alloy blank in step 2) is 0.1-0.3 mm.
[0022] According to the above scheme, the specific steps of step 3) are as follows: use a coating machine to spin-coat PMMA electron beam photoresist on the upper and lower surfaces of the copper foil, bake it in an oven at 180-200°C for 1-2 hours, then cover the surface of the copper foil with a circular grid mask, and then use an electron beam lithography machine to expose the PMMA electron beam photoresist on the upper surface of the copper foil, and then use a developer to develop it to leave the mask pattern on the copper foil, then immerse the copper foil in a ferric chloride solution for etching, and after the etching is completed, remove the remaining PMMA electron beam photoresist on the surface of the copper foil to obtain a metal copper mesh skeleton.
[0023] According to the above scheme, the developer is a mixture of methyl isobutyl ketone (MIBK) and isopropyl alcohol (IPA) in a volume ratio of 1:3.
[0024] According to the above scheme, the concentration of the ferric chloride solution in step 3) is 1 to 1.8 mol / L, preferably 1 to 1.5 mol / L.
[0025] According to the above scheme, in step 3), the diameter of the circles on the circular grid mask is 50-300 μm, and the circular spacing is 10-30 μm.
[0026] According to the above scheme, the etching process conditions in step 3) are: constant temperature etching at 40-50°C for 0.5-2h.
[0027] According to the above scheme, the method of step 3) removing the PMMA electron beam photoresist remaining on the surface of the copper foil is: immersing the copper foil in acetone at a constant temperature of 45 to 60° C. to react until the PMMA electron beam photoresist is completely removed.
[0028] According to the above scheme, the pressing process conditions in step 4) are: pressure 1-5 MPa, and holding time 1-2 min.
[0029] According to the above scheme, the debinding process conditions in step 4) are: in a nitrogen-hydrogen mixed atmosphere (wherein hydrogen accounts for 5% by volume), the temperature is increased from room temperature to 600-850°C at a heating rate of 0.3-1°C / min, and kept at this temperature for 2-4h.
[0030] According to the above scheme, the sintering process conditions in step 4) are: vacuum degree 10 -2 ~10 -1 Pa, heated to 850-900℃ at room temperature at a rate of 1-3℃ / min, kept warm for 30-50min, then began to pressurize, the pressure was 30-50MPa, and at the same time heated to 980-1050℃ at a rate of 0.5-1℃ / min, kept warm for 10-30min, then kept cool to 800-950℃ and kept warm again for 120-240min, and released the pressure after sintering. Sintering is carried out in a hot press sintering furnace or an SPS sintering furnace to densify the material, with a density of 98.5-99.0%.
[0031] The present invention also includes an ultra-thin high thermal conductivity copper-diamond composite material prepared according to the above method, wherein the ultra-thin high thermal conductivity copper-diamond composite material has a sandwich structure, wherein the middle layer is a copper-diamond composite material layer, and the upper and lower layers are copper alloy material layers, wherein the copper-diamond composite material layer is obtained by filling boron-plated diamond particles in a copper foil having circular through holes distributed in an array, and the gaps between the diamond particles are densely filled with copper alloy.
[0032] According to the above scheme, the thickness of the copper-diamond composite material layer is 0.05-0.3 mm, and the thickness of the ultra-thin high thermal conductivity copper-diamond composite material is 0.2-0.4 mm.
[0033] The present invention also includes the application of the ultra-thin high thermal conductivity copper-diamond composite material in the fields of packaging materials and heat dissipation materials.
[0034] Diamond particles have a large specific surface area and high surface energy, making it difficult to achieve high-strength composites with other materials. Since the strength of covalent bonds (such as BC) is usually stronger than that of ionic bonds (such as Ti-C), the use of diamond-like elements B to wrap diamond particles to form a "BC diamond" structure will have a more stable interface structure and better performance than using transition metals (such as "Ti-C diamond"). The interface bonding strength between diamond and copper has not been solved. The present invention uses a vacuum micro-evaporation coating method to prepare a boron coating on the surface of diamond. The process is as follows:
[0035] 4 H3BO3 → 2 B2O3 + 6H2O (1)
[0036] 4B+3O2→2B2O3 (2)
[0037] 7C(s) + 2B2O3 (l,g) → B4C + 6CO (g) (3)
[0038] 2B2O3+6Mg+C →B4C+6MgO (4)
[0039] At present, the copper mesh adopts the warp and weft copper wire weaving process, and its thickness and period cannot be very small due to the limitation of the copper wire diameter. The present invention etches the copper foil into a precision copper mesh with regular arrangement by wet etching, and then arranges the boron-plated diamond particle array in the copper mesh to form a copper diamond skeleton. The diamond skeleton is to prevent the diamond particles from being offset due to force during the sintering and pressing process, so as to ensure the processability of the copper diamond surface.
[0040] The copper alloy blank prepared by the tape casting method has uniform composition, good thickness consistency and certain plasticity. The copper diamond skeleton is fixed in the middle and then pressed to form a copper diamond composite material with a "sandwich structure". Since the copper alloy powder contains a certain amount of B, Ti, Cr, Zr and other elements, these elements play a certain activation role to reduce the melting point of the copper alloy and improve the fluidity of the copper alloy. During the sintering process, the molten copper alloy will penetrate into the skeleton to bond the diamond and copper together. The alloy elements diffuse into each other under the action of the concentration gradient to form a solid solution, which enhances the bonding strength between diamond and copper and improves the thermal conductivity of the interface.
[0041] In addition, through high-temperature pressure sintering, the density of the copper-diamond composite material is increased by external force to achieve complete density, and the bonding strength of copper and diamond is strengthened. After sintering, sufficient insulation time is given at 800-950°C to allow the elements to fully diffuse, thereby improving the thermal conductivity and mechanical properties of the composite material.
[0042] The beneficial effects of the present invention are:
[0043] 1. The copper-diamond composite material provided by the present invention has good thermal conductivity (>480W / mK), ultra-thin thickness of 0.2-0.4mm, light density, roughness Ra<0.2, and the upper and lower surfaces are copper alloys, with a sandwich structure and good surface machinability, and is suitable for the fields of miniaturization and lightweight electronic components;
[0044] 2. The present invention adopts the tape casting process to conveniently control the thickness of the film, has high production efficiency, low process cost, and is suitable for industrial application. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 The surface and cross-sectional SEM images of the boron-coated diamond particles obtained in step 1) of Example 1;
[0046] Figure 2 A comparison photo of the ultra-thin high thermal conductivity copper-diamond composite material prepared in Example 2 and a coin;
[0047] Figure 3 This is a schematic diagram of the cross-sectional structure of the ultra-thin high thermal conductivity copper-diamond composite material prepared in Example 2. DETAILED DESCRIPTION
[0048] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below with reference to the accompanying drawings.
[0049] The copper alloy powder used in the examples and comparative examples of the present invention is vacuum atomized powder, has a particle size of 3-5 μm, and contains: 0.98 wt% B, 0.42 wt% Ti, 0.73 wt% Cr, 0.31 wt% Zr, and the balance is Cu.
[0050] Example 1
[0051] A method for preparing ultra-thin high thermal conductivity copper diamond composite material by tape casting, the process flow chart is as follows Figure 1 As shown, the specific steps are as follows:
[0052] 1) boron-plating the surface of diamond particles: 45wt.% diamond particles (particle size 100μm), 20wt.% boron powder (particle size 1-5μm), 32wt.% boric acid powder (particle size 20-25μm), and 3wt.% magnesium powder (particle size 10-20μm) are uniformly stirred and laid in an alumina ceramic crucible, and then the ceramic crucible is placed in a high-temperature tube furnace, heated to 1350°C at a heating rate of 3°C / min at room temperature for 45min, cooled, and washed to obtain boron-plated diamond particles;
[0053] 2) Preparation of copper alloy casting green billet: Raw materials and mass percentage are as follows: copper alloy powder 63wt.%, glyceryl tristearate 1.0wt.%, phenolic resin (purchased from Hebei Zetian Chemical Co., Ltd., 2123D1 type)
[0054] 1.2wt.%, polyvinyl alcohol (Sinopec, PVA092-20) 1.3wt.%, glycerol 1.5wt.%, dioctyl phthalate 1wt.%, butanone 26wt.% and trichloroethylene 5wt.%, the above raw materials are ball-milled and mixed for 6h, the slurry obtained by ball milling is defoamed and filtered to obtain copper alloy tape-casting slurry, the obtained copper alloy tape-casting slurry is injected into a tape-casting machine, the height of the scraper is 0.2mm, the speed of the tape-casting machine is controlled to be 80cm / min, and the copper alloy blank with a thickness of 0.2mm is obtained after drying in the shade;
[0055] 3) Preparation of a metal copper mesh skeleton: using a coating machine to spin-coat PMMA electron beam photoresist on the upper and lower surfaces of a copper foil with a thickness of 0.08 mm, and baking in an oven at 180° C. for 1 h, and then covering the copper foil surface with a circular grid mask (with a circular diameter of 100 μm and a circular spacing of 15 μm), and then using an electron beam lithography machine to expose the PMMA electron beam photoresist on the upper surface of the copper foil, and then using a developer (volume ratio of methyl isobutyl ketone: isopropanol = 1:3) for development to leave the mask pattern on the copper foil, and then immersing the copper foil in a 45° C. ferric chloride solution (concentration 1.2 mol / L) for etching for 0.5 h. After the etching is completed, the copper foil is immersed in 45° C. acetone to remove the remaining PMMA electron beam photoresist on the copper foil surface to obtain a metal copper mesh skeleton;
[0056] 4) Preparing an ultra-thin copper diamond raw blank: cutting the copper alloy blank and the metal copper mesh skeleton into the same size, placing a layer of copper alloy blank on the bottom layer, and then covering it with a layer of metal copper mesh skeleton and laying the boron-plated diamond particles obtained in step 1) inside the metal copper mesh skeleton, ensuring that each copper mesh hole is filled with boron-plated diamond particles, and then removing excess boron-plated diamond particles with a scraper, and finally covering the upper surface with a layer of copper alloy blank, pressing the stacked sample with a hydraulic press at a pressure of 3 MPa for 1 min, and obtaining an ultra-thin copper diamond raw blank with a "copper alloy-copper diamond-copper alloy" sandwich structure;
[0057] 5) Debinding sintering: The ultra-thin copper diamond raw material was subjected to debinding treatment in a nitrogen-hydrogen mixed atmosphere (where hydrogen accounts for 5% by volume): the temperature was raised to 850°C at a heating rate of 0.5°C / min at room temperature and kept at that temperature for 4 hours. After debinding, it was placed in a hot pressing sintering furnace for dense sintering: the vacuum degree was 8×10 -2Pa, during the heating process, it is heated from room temperature to 850°C at a rate of 3°C / min, kept warm for 30 minutes, and then pressurized with a pressure of 45MPa. At the same time, it is heated to 1030°C at a rate of 1°C / min, kept warm for 30min, and then cooled to 950°C with pressure maintained and kept warm for 240min. After sintering, the pressure is released, and finally a 0.2mm thick ultra-thin high thermal conductivity copper-diamond composite material is obtained after grinding and polishing, with a thermal conductivity of 482W / mK, a thermal expansion coefficient of 6.8ppm / °C, a surface roughness Ra=0.13, and a density of 98.8%.
[0058] like Figure 1 The surface and cross-sectional SEM images of the boron-coated diamond particles obtained in step 1) of this embodiment are shown. It can be seen that the diamond surface is completely covered by a uniform coating with a thickness of about 1 μm. The coating is rough, which can increase the specific surface area of the diamond.
[0059] Example 2
[0060] A method for preparing an ultra-thin high thermal conductivity copper-diamond composite material by tape casting, the specific steps are as follows:
[0061] 1) boron-plating the surface of diamond particles: 40wt.% diamond particles (particle size 300μm), 17wt.% boron powder (particle size 1-5μm), 40wt.% boric acid powder (particle size 20-25μm), and 3wt.% magnesium powder (particle size 10-20μm) are stirred evenly and laid in an alumina ceramic crucible, and then the ceramic crucible is placed in a high-temperature tube furnace, heated to 1450°C at a heating rate of 3°C / min at room temperature for 45min, cooled, and washed to obtain boron-plated diamond particles (coating thickness 1μm);
[0062] 2) Preparation of copper alloy tape casting blank: raw materials and mass percentage are as follows: 63wt.% copper alloy powder, 1.0wt.% glycerol tristearate, 1.2wt.% phenolic resin (purchased from Hebei Zetian Chemical Co., Ltd., 2123D1 type), 1.3wt.% polyvinyl alcohol (Sinopec, PVA092-20), 1.5wt.% glycerol, 1wt.% dioctyl phthalate, 26wt.% butanone and 5wt.% trichloroethylene. The above raw materials are ball-milled and mixed for 6h. The slurry obtained by ball milling is defoamed and filtered to obtain copper alloy tape casting slurry. The obtained copper alloy tape casting slurry is injected into a tape casting machine with a scraper height of 0.3mm and a tape casting machine speed of 60cm / min. After drying in the shade, a copper alloy blank with a thickness of 0.3mm is obtained.
[0063] 3) Preparation of a metal copper mesh skeleton: using a coating machine to spin-coat PMMA electron beam photoresist on the upper and lower surfaces of a copper foil with a thickness of 0.2 mm, and baking in an oven at 180° C. for 1 h, and then covering the copper foil surface with a circular grid mask (with a circular diameter of 300 μm and a circular spacing of 20 μm), and then using an electron beam lithography machine to expose the PMMA electron beam photoresist on the upper surface of the copper foil, and then using a developer (volume ratio of methyl isobutyl ketone: isopropanol = 1:3) for development to leave the mask pattern on the copper foil, and then immersing the copper foil in a 45° C. ferric chloride solution (concentration 1.5 mol / L) for etching for 1 h, and after the etching is completed, immersing the copper foil in 45° C. acetone to remove the remaining PMMA electron beam photoresist on the copper foil surface to obtain a metal copper mesh skeleton;
[0064] 4) Preparing a copper-diamond composite material raw blank: cutting the copper alloy blank and the metal copper mesh skeleton into the same size, placing a layer of copper alloy blank on the bottom layer, and then covering it with a layer of metal copper mesh skeleton and laying the boron-plated diamond particles obtained in step 1) inside the metal copper mesh skeleton, ensuring that each copper mesh hole is filled with boron-plated diamond particles, and then removing excess boron-plated diamond particles with a scraper, and finally covering the upper surface with a layer of copper alloy blank, pressing the stacked sample with a hydraulic press at a pressure of 3 MPa for 1 min, to obtain an ultra-thin copper diamond raw blank with a "copper alloy-copper diamond-copper alloy" sandwich structure.
[0065] 5) Debinding sintering: The ultra-thin copper diamond raw material was subjected to debinding treatment in a nitrogen-hydrogen mixed atmosphere (where hydrogen accounts for 5% by volume): the temperature was raised to 850°C at a heating rate of 0.5°C / min at room temperature and kept at that temperature for 4 hours. After debinding, it was placed in an SPS sintering furnace for dense sintering: the vacuum degree was 2×10 -2 Pa, during the heating process, it is heated from room temperature to 850℃ at a rate of 3℃ / min, kept warm for 30min, and then pressurized with a pressure of 35MPa. At the same time, it is heated to 1000℃ at a rate of 1℃ / min, kept warm for 30min, and then cooled to 900℃ with pressure maintained for 240min. After sintering, the pressure is released.
[0066] 6) Grinding and polishing: After final grinding and polishing, a 0.4 mm thick ultra-thin high thermal conductivity copper diamond composite material is obtained, with a thermal conductivity of 563 W / mK, a thermal expansion coefficient of 6.4 ppm / °C, a surface roughness Ra=0.12, and a density of 98.6%.
[0067] Figure 2 This is a comparison photo of the ultra-thin high thermal conductivity copper-diamond composite material prepared in this embodiment and a coin. It can be seen that the prepared copper-diamond composite material is an ultra-thin and dense disc.
[0068] Figure 3Schematic diagram of the cross-sectional structure of the ultra-thin high thermal conductivity copper-diamond composite material prepared in this embodiment.
[0069] Comparative Example 1-2
[0070] The temperature of boron plating on the diamond surface in step 1) of Example 1 was changed, and the other conditions were the same as those of Example 1. The ultra-thin high thermal conductivity copper-diamond composite materials prepared in Comparative Examples 1-2 and Example 1 were compared, and the results are shown in Table 1.
[0071] Table 1
[0072]
[0073] Comparative Examples 3-4
[0074] The mass of copper alloy in step 2) of Example 1 is changed, and the other conditions are the same as those of Example 1. The castability and performance after debinding treatment of the copper alloy tape casting slurries prepared in Comparative Examples 3-4 and Example 1 are compared. The results are shown in Table 2.
[0075] Table 2
[0076]
[0077] Comparative Examples 5-7
[0078] The debinding process of the copper-copper diamond raw embryo in Example 1 was changed, and the other conditions were the same as those in Example 1. The performance after debinding of Comparative Examples 5-7 and Example 1 was compared. The results are shown in Table 3.
[0079] Table 3
[0080] sample Debinding temperature Heating rate Debinding time result Example 1 850℃ 0.5℃ / min 4h The temperature is suitable and the adhesive is removed cleanly Comparative Example 5 400℃ 0.5℃ / min 4h The temperature is too low and there is adhesive residue. Comparative Example 6 800℃ 3℃ / min 4h The heating speed is too fast, and the copper diamond raw embryo cracks Comparative Example 7 800℃ 0.5℃ / min 1h The debonding time is too short and there is adhesive residue.
[0081] Comparative Examples 8-11
[0082] The hot pressing sintering parameters in Example 1 were changed, and the other conditions were the same as those in Example 1. The ultra-thin high thermal conductivity copper diamond composite materials prepared in Examples 8-11 and Example 1 were subjected to comparative tests. The results are shown in Table 4.
[0083] Table 4
[0084]
[0085] From the comparison of Tables 1-4 above, it can be seen that diamond boron plating temperature, tape casting slurry ratio, debinding process conditions, and sintering process conditions will all have an impact on product performance.
Claims
1. A method for preparing an ultra-thin high thermal conductivity copper-diamond composite material by tape casting, characterized in that: The specific steps are as follows: 1) boron-plating the surface of diamond particles: diamond particles, boron powder, boric acid powder and magnesium powder are uniformly stirred to obtain a mixed powder, which is laid in an alumina ceramic crucible, and then the alumina ceramic crucible is placed in a high-temperature tube furnace for heat treatment, and after cooling, the crucible is taken out and cleaned to obtain boron-plated diamond particles; 2) preparing copper alloy tape casting blank: copper alloy powder, dispersant, binder, plasticizer and organic solvent are ball-milled for 4-8 hours, the slurry obtained by ball milling is defoamed and filtered to obtain copper alloy tape casting slurry, and the obtained copper alloy tape casting slurry is injected into a tape casting machine for tape casting to obtain copper alloy blank; 3) preparing a metal copper mesh skeleton: using a copper foil with a thickness of 0.05 to 0.3 mm to be wet-etched to obtain a metal copper mesh skeleton with regularly arranged circular through holes; 4) Preparing an ultra-thin high thermal conductivity copper-diamond composite material: cutting the copper alloy blank prepared in step 2) and the metal copper mesh skeleton prepared in step 3) into the same size, then using a layer of copper alloy blank as the bottom layer, then covering a layer of metal copper mesh skeleton and laying the boron-coated diamond particles obtained in step 1) inside the metal copper mesh skeleton, ensuring that each mesh of the metal copper mesh skeleton is filled with boron-coated diamond particles, and finally covering the upper surface of the metal copper mesh skeleton with a layer of copper alloy blank, pressing the stacked sample into shape, and then removing binder, sintering, and polishing to obtain an ultra-thin high thermal conductivity copper-diamond composite material.
2. The method for preparing an ultra-thin high thermal conductivity copper-diamond composite material by tape casting according to claim 1, characterized in that: Step 1) The diamond particles have a particle size of 100 to 300 μm; the boron powder has a particle size of 1 to 5 μm; the boric acid powder has a particle size of 20 to 30 μm; and the magnesium powder has a particle size of 10 to 20 μm; the mass percentage of each component in the mixed powder of step 1) is as follows: 40 to 45% diamond particles, 10 to 20% boron powder, 30 to 40% boric acid powder, and 2 to 5% magnesium powder.
3. The method for preparing an ultra-thin high thermal conductivity copper-diamond composite material by tape casting according to claim 1, characterized in that: The heat treatment process conditions of step 1) are: heating to 1100-1500° C. at a heating rate of 3-15° C. / min at room temperature, and keeping warm for 30-60 minutes; the boron coating thickness of the boron-coated diamond particles in step 1) is 800-1200 nm.
4. The method for preparing an ultra-thin high thermal conductivity copper-diamond composite material by tape casting according to claim 1, characterized in that: Step 2) The copper alloy powder is vacuum atomized powder, with a particle size of 3-10 μm, and the composition and mass percentage are: B 0.50-1.20%, Ti 0.15-0.55%, Cr 0.50~0.80%, Zr0.25~0.45%, and the balance is Cu; step 2) the dispersant is a mixture of one or more of glycerol tristearate, phosphate or triethanolamine, the binder is a mixture of one or more of phenolic resin, ethyl cellulose, polyvinyl alcohol or polyvinyl butyral, the plasticizer is a mixture of one or more of glycerol, dioctyl phthalate, polyethylene glycol or propylene glycol, and the organic solvent is a mixture of one or more of butanone, trichloroethylene, isopropyl alcohol or ethyl lactate; step 2) the mass percentages of the copper alloy powder, dispersant, binder, plasticizer and organic solvent are as follows: copper alloy powder 60~70%, dispersant 1~3%, binder 2~5%, plasticizer 2~4%, organic solvent 20~35%.
5. The method for preparing an ultra-thin high thermal conductivity copper-diamond composite material by tape casting according to claim 1, characterized in that: Step 3) The specific steps are as follows: use a coating machine to spin-coat PMMA electron beam photoresist on the upper and lower surfaces of the copper foil, bake it in an oven at 180-200° C. for 1-2 hours, then cover the surface of the copper foil with a circular grid mask, and then use an electron beam lithography machine to expose the PMMA electron beam photoresist on the upper surface of the copper foil, and then use a developer to develop it to leave the mask pattern on the copper foil, then immerse the copper foil in a ferric chloride solution for etching, and after the etching is completed, remove the remaining PMMA electron beam photoresist on the surface of the copper foil to obtain a metal copper mesh skeleton.
6. The method for preparing an ultra-thin high thermal conductivity copper-diamond composite material by tape casting according to claim 5, characterized in that: The circular diameter on the circular grid mask is 50 to 300 μm, and the circular spacing is 10 to 30 μm; The etching process conditions are: constant temperature etching at 40-50° C. for 0.5-2 h; the method for removing the remaining PMMA electron beam photoresist on the surface of the copper foil is: immersing the copper foil in constant temperature acetone at 45-60° C. to react until the PMMA electron beam photoresist is completely removed.
7. The method for preparing an ultra-thin high thermal conductivity copper-diamond composite material by tape casting according to claim 1, characterized in that: Step 4) The pressing process conditions are: pressure 1-5 MPa, holding time 1-2 min; Step 4) The debinding process conditions are: in a nitrogen-hydrogen mixed atmosphere, heating from room temperature to 600-850°C at a heating rate of 0.3-1°C / min, and keeping warm for 2-4 h.
8. The method for preparing an ultra-thin high thermal conductivity copper-diamond composite material by tape casting according to claim 1, characterized in that: Step 4) Sintering process conditions: vacuum degree 10 -2 ~10 -1 Pa, heat to 850-900°C at a rate of 1-3°C / min at room temperature, keep warm for 30-50min, then start pressurizing with a pressure of 30-50MPa, and heat to 980-1050°C at a rate of 0.5-1°C / min, keep warm for 10-30min, then cool down to 800-950°C while maintaining the pressure and keep warm for another 120-240min, and release the pressure after sintering is completed.
9. The ultra-thin high thermal conductivity copper-diamond composite material prepared by the method according to any one of claims 1 to 8, characterized in that: The ultra-thin high thermal conductivity copper-diamond composite material has a sandwich structure, wherein the middle layer is a copper-diamond composite material layer, and the upper and lower layers are copper alloy material layers. The copper-diamond composite material layer is obtained by filling boron-plated diamond particles in a copper foil with circular through holes distributed in an array, and the gaps between the diamond particles are densely filled with copper alloy.
10. Application of the ultra-thin high thermal conductivity copper-diamond composite material according to claim 9 in the fields of packaging materials and heat dissipation materials.
Citation Information
Patent Citations
Method for coating surface of diamond / copper composite material with copper
CN112974809A
Cited By
Preparation method and application of copper diamond copper-clad layer grafting fin
CN122644605A
Diamond-metal composite material having six sides coated with metal, and processing method therefor and use thereof
WO2026081537A1