Surface modified kovar powder reinforced copper-based composite material and preparation method thereof

By plating the cladding layer on the surface of the Cova powder and using hot press sintering technology, the problem of interface diffusion in the Cova copper composite is solved, which significantly improves its thermal conductivity and improves the life and reliability of the device.

CN118910461APending Publication Date: 2024-11-08CENT SOUTH UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410977534.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

When preparing Cova copper composites, the interface diffusion between Cova alloy and copper leads to a decrease in thermal conductivity, affecting the thermal conductivity of the material and the life and reliability of the device.

Method used

The cladding layer is coated on the surface of the Cova powder by vacuum high-temperature treatment, and the surface-modified Cova powder reinforced copper-based composite material is prepared by using hot pressing and sintering technology to inhibit the diffusion of interface elements and improve thermal conductivity.

Benefits of technology

It effectively inhibits the diffusion of interface elements of Kerva copper composite material, significantly improves its thermal conductivity, and improves the life and reliability of high-power and high-integrated devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910461A_ABST
    Figure CN118910461A_ABST
Patent Text Reader

Abstract

The invention relates to a kovar copper composite material and a preparation method thereof, and belongs to the technical field of design and preparation of kovar powder reinforced copper-based composite materials. The surface modified Kovar powder reinforced copper-based composite material comprises a Kovar alloy, a coating layer and a copper alloy, the Kovar alloy is coated with the coating layer, the Kovar alloy coated with the coating layer is evenly distributed in the copper alloy, and the coating layer is a tungsten-containing coating layer. The preparation method comprises the steps that firstly, tungsten powder and kovar powder are mixed and then subjected to vacuum high-temperature treatment, completely-coated kovar powder is obtained, then the completely-coated kovar powder is mixed with copper powder, hot pressing sintering forming is conducted, and the surface-modified kovar powder reinforced copper-based composite material is obtained. The surface-modified kovar powder is adopted, element diffusion between the kovar alloy powder and a copper matrix can be effectively prevented, and therefore the prepared kovar copper composite material has good heat conductivity. The material is reasonable in structural design, simple and controllable in process and convenient for industrial application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a kovar-copper composite material and a preparation method thereof, belonging to the technical field of design and preparation of kovar powder reinforced copper-based composite materials. Background Art

[0002] With the rapid development of the microelectronics industry, higher requirements have been put forward for the thermal conductivity of both sealing materials and electronic packaging heat sink materials. However, the thermal conductivity of Kovar alloy is poor. Although pure Kovar alloy is still used as a high-power glass high-sealing material and a high-integration electronic packaging material, long-term service will lead to high-temperature failure of the sealing solder joints or overheating of electronic components, which will cause the efficiency to decrease, seriously affecting the life and reliability of the device. Metal Cu is the metal material with the best electrical and thermal conductivity except Ag. By making Cu and Kovar alloy into a composite material, we can obtain the advantages of Kovar alloy such as low expansion and strong weldability, and make the material as a whole obtain excellent electrical and thermal conductivity. Therefore, Kovar / copper composite materials can solve the contradiction between the low thermal expansion coefficient and high thermal conductivity of pure Kovar alloy, and will greatly improve the life and reliability of high-power and highly integrated devices.

[0003] The difficulty in preparing Kovar copper composite materials lies in the fact that the iron, cobalt and nickel elements in Kovar alloy, especially nickel, have a very high solid solubility in copper. During the high-temperature sintering process of the composite material, interfacial diffusion will occur between the Kovar alloy and copper. After the solute atoms enter the copper matrix, the thermal conductivity of copper will be greatly reduced, thereby reducing the thermal conductivity of the composite material. Therefore, how to inhibit the interfacial diffusion between Kovar and copper in Kovar copper composite materials is the key to preparing high thermal conductivity Kovar copper composite materials. Summary of the invention

[0004] Aiming at the problem of how to suppress the interface diffusion between Kovar alloy and copper matrix, the present invention designs and proposes a surface modified Kovar powder reinforced copper matrix composite material and develops a method for surface coating of Kovar powder by vacuum high temperature treatment, and a method for preparing a composite material by hot pressing and sintering the treated Kovar powder and copper powder.

[0005] The thermal conductivity of the surface modified Kovar powder reinforced copper-based composite material designed and prepared by the present invention is greatly improved. The present invention effectively inhibits the diffusion of interface elements of the Kovar copper composite material.

[0006] Specifically, the method comprises the following steps: first vacuum coating kovar powder to form a coating layer on the surface of the kovar powder, and then hot pressing and sintering to obtain a surface-coated kovar copper composite material.

[0007] The invention discloses a surface modified kovar powder reinforced copper-based composite material, which comprises a kovar alloy, a coating layer and copper. The coating layer is coated on the kovar alloy, the kovar alloy coated with the coating layer is uniformly distributed in the copper, and the coating layer is a tungsten-containing coating layer.

[0008] The invention discloses a preparation method of a surface modified kovar powder reinforced copper-based composite material. Firstly, tungsten powder and kovar powder are mixed and then subjected to vacuum high-temperature treatment, the high-temperature treated kovar powder and tungsten powder are separated to obtain a completely coated kovar powder, which is then mixed with copper powder and hot-pressed and sintered to obtain a kovar-copper composite material with no interface diffusion and high thermal conductivity.

[0009] Therefore, the present invention provides the following technical solution: a method for preparing a surface-modified kovar powder reinforced copper-based composite material, comprising the following steps:

[0010] Step 1: According to the mass ratio of tungsten powder to kovar alloy powder = 3-5, weigh tungsten powder and kovar alloy powder and mix them thoroughly; the particle size of the tungsten powder used is less than or equal to 0.1d; the d is the particle size of the kovar alloy powder;

[0011] Step 2: Place the mixed powder in a vacuum furnace for high temperature treatment; the high temperature treatment temperature is 1050°C to 1100°C; the heat preservation time is 2 to 5 hours;

[0012] Step 3: Separating the tungsten / Kovar mixed powder after high temperature treatment to obtain Kovar alloy powder with a coating layer;

[0013] Step 4: weigh the Kovar alloy powder with a coating layer and the copper powder and mix them thoroughly according to the mass ratio of Kovar alloy powder with a coating layer: copper powder = 40-80:60-20; obtain Kovar-copper composite powder;

[0014] Step 5: Load the Kovar-copper composite powder into a mold and perform vacuum hot pressing and sintering to obtain a surface-modified Kovar powder-reinforced copper-based composite material.

[0015] The mass ratio of the tungsten powder to the kovar powder in step 1 is 3 to 5, preferably 4 to 5. Too low a mass ratio will result in an incomplete coating layer.

[0016] Preferably, the particle size of the kovar powder in step one is 80-300 μm, and the particle size of the tungsten powder is 1-5 μm.

[0017] The invention uses large-size kovar powder and small-size tungsten powder not only to facilitate the subsequent separation of the two using a screen, but also to control the particle size of the tungsten powder to be less than or equal to 0.1d and to match the mass ratio of the two so that the tungsten powder can be evenly coated.

[0018] The conditions of the vacuum high temperature treatment in step 2 are: insulation temperature 1050°C to 1100°C; insulation time 2 to 5 hours, preferably 4 to 5 hours; vacuum degree 9×10 -3 ~2×10 -2 Pa; cooling with the furnace. Too low temperature will lead to incomplete coating or even coating failure, too high temperature will cause sintering of tungsten powder and cannot separate mixed powder, too long time will lead to too thick coating and affect the ductility, too short time will lead to incomplete coating.

[0019] In the present invention, in step 3, the tungsten / kovar mixed powder after high temperature treatment is separated by sieve to obtain the kovar alloy powder with complete coating. The mesh number of the sieve used is 200 mesh. The reason why the present invention chooses the sieve with a mesh number of 200 is that this is the largest sieve that can separate the kovar powder and the tungsten powder, and with the vibration screening, it can further ensure that the kovar alloy powder (screened material) with complete coating is obtained.

[0020] The complete coating of the Kovar alloy powder described in step 3 is a tungsten-iron compound.

[0021] In the kovar copper composite powder described in step 4, the mass percentage of the kovar alloy powder with the coating layer is 40% to 80%.

[0022] The hot pressing sintering conditions described in step five are: temperature of 750-950°C, preferably 800-950°C, more preferably 800-910°C; holding time of 10-30min, preferably 20-30min; heating rate of 30-50°C / min; pressure of 30-50MPa.

[0023] In step five, the mold used is preferably a carbon mold, and more preferably a graphite mold.

[0024] In the present invention, when the mass ratio of the kovar alloy with the coating layer to copper is 6:4, the density of the obtained kovar-copper composite material is 8.31-8.35 g·cm -3 , density is greater than or equal to 99%, thermal conductivity is 85~86W·m -1 ·K -1 The thermal expansion coefficient from room temperature to 150°C is (9.6~9.8)×10 -6 K -1 .

[0025] In the present invention, when the mass ratio of the kovar alloy with the coating layer to copper is 7:3, the density of the obtained kovar-copper composite material is 8.2-8.25 g·cm -3 , density is greater than or equal to 98.5%, thermal conductivity is 66~67W·m -1 ·K -1The thermal expansion coefficient from room temperature to 150°C is (8.7~8.9)×10 -6 K -1 .

[0026] In the present invention, when the mass ratio of the kovar alloy with the coating layer to copper is 8:2, the density of the obtained kovar-copper composite material is 8.1-8.15 g·cm -3 , density is greater than or equal to 98.5%, thermal conductivity is 55~55.6W·m -1 ·K -1 The thermal expansion coefficient from room temperature to 150°C is (8.2~8.4)×10 -6 K -1 .

[0027] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0028] (1) The present invention uses a vacuum high-temperature treatment method to plate the surface of the kovar powder, which has strong controllability of process parameters and low cost.

[0029] (2) The kovar powder coating prepared by the present invention is complete, which effectively inhibits the interface diffusion between the kovar alloy powder and the copper matrix, so that the prepared kovar-copper composite material has high thermal conductivity. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 The following are the actual photograph and SEM image of the kovar powder before and after plating in Example 1.

[0031] Figure 2 1. The SEM image and interface element distribution diagram of the kovar copper composite material prepared in Example 1.

[0032] Figure 3 These are the SEM images and interface element distribution diagrams of the Kovar copper composite material prepared in Comparative Example 1.

[0033] Figure 4 This is the SEM morphology of the plated kovar powder obtained in Comparative Examples 2-4.

[0034] from Figure 1 It can be seen that the surface of the plated kovar powder is completely covered by the coating.

[0035] from Figure 2 It can be seen that the coating on the surface of the Kovar powder is complete and there is no obvious interdiffusion of interface elements at the interface of the composite material.

[0036] from Figure 3 It can be seen that there is serious element diffusion at the interface in the unplated Kovar copper composite.

[0037] from Figure 4It can be seen that in the vacuum coating process, a too low ratio of tungsten powder to kovar powder, too low temperature and too short processing time will lead to incomplete surface coating of kovar powder. DETAILED DESCRIPTION

[0038] The Kovar alloy used in the embodiments and comparative examples of the present invention is 4J29 Kovar alloy.

[0039] Example 1

[0040] In this embodiment 1, a fully plated Kovar alloy powder and a Kovar-copper composite material having a fully plated Kovar alloy mass fraction of 60% and a copper mass fraction of 40% are pre-prepared. The preparation process includes the following steps:

[0041] (1) Preparation and mixing of Kovar powder and tungsten powder

[0042] Weigh 100g of Kovar alloy powder with a particle size of 80-300μm. Its microstructure is as shown in the attached figure. Figure 1 As shown in a, take 500 g of tungsten powder with a particle size of 1 to 5 μm, mix it evenly and put it into a corundum crucible for later use.

[0043] (2) High temperature treatment in vacuum furnace

[0044] The powder in the corundum crucible in step (1) was placed in a vacuum furnace at a temperature of 1100°C and a vacuum degree of 9×10 - 3 After keeping warm for 4 hours under the condition of 1.577 Pa, it is cooled with the furnace.

[0045] (3) Separation of Kovar powder and tungsten powder after plating

[0046] The mixed powder after vacuum high temperature treatment in step (2) is separated by a sieve with a mesh size of 200, and the powder on the sieve is taken to obtain the plated kovar powder, the microstructure of which is shown in the attached figure. Figure 1 As shown in b.

[0047] (4) Preparation of composite powder

[0048] According to the proportion, take 60g of the plated kovar powder obtained in step (3), and weigh 40g of copper powder with an average particle size of 10μm, and mix them evenly to obtain kovar-copper composite powder.

[0049] (5) Hot pressing sintering

[0050] The Kovar composite powder in step (4) was placed in a graphite mold and sintered on a hot press at a temperature of 800°C, a holding time of 30 min, a heating rate of 30°C / min, and a pressure of 40 MPa. After cooling and demoulding, the Kovar copper composite material was obtained. The SEM microstructure and element distribution at the interface are shown in the attached figure. Figure 2shown.

[0051] The performance of the kovarable copper composite material obtained in Example 1 was tested, including density, thermal conductivity and thermal expansion coefficient, wherein the density was tested by using the Archimedes drainage method to measure the actual density, and the ratio of the actual density to the theoretical density was the density. The thermal conductivity was tested by using a laser thermal conductivity meter to measure the thermal diffusion coefficient of the composite material, and the product of the thermal diffusion coefficient, density and specific heat capacity was the thermal conductivity of the composite material. The thermal expansion coefficient was tested by using a thermal expansion meter to directly test and obtain the result.

[0052] The test results are as follows:

[0053] The density of the prepared kovar copper composite material is 8.33 g·cm -3 , density is 99.1%, thermal conductivity is 85.4W·m -1 ·K -1 , thermal expansion coefficient (room temperature to 150°C) is 9.8×10 -6 K -1 .

[0054] Example 1-1, other conditions are the same as Example 1, only the sintering temperature is changed to 900 ° C, the density of the composite material after sintering is 8.36 g cm -3 , density is 99.4%, thermal conductivity is 87.5W·m -1 ·K -1 , thermal expansion coefficient (room temperature to 150°C) is 9.8×10 -6 K -1 .

[0055] Example 1-2, other conditions are the same as Example 1, only the holding time is changed to 20min, the density of the composite material after sintering is 8.29g·cm -3 , density is 98.6%, thermal conductivity is 82.9W·m -1 ·K -1 , thermal expansion coefficient (room temperature to 150°C) is 9.8×10 -6 K -1 .

[0056] In Example 1-3, other conditions were the same as in Example 1, except that the sintering pressure was changed to 50 MPa. The density of the composite material after sintering was 8.35 g·cm -3 , density is 99.3%, thermal conductivity is 86.8W·m -1 ·K -1 , thermal expansion coefficient (room temperature to 150°C) is 9.8×10 -6 K -1 .

[0057] Example 2

[0058] In this embodiment 2, a fully plated Kovar alloy powder and a Kovar-copper composite material having a fully plated Kovar alloy mass fraction of 70% and a copper mass fraction of 30% are pre-prepared. The preparation process includes the following steps:

[0059] (1) Preparation and mixing of Kovar powder and tungsten powder

[0060] Weigh 100 g of kovar powder with a particle size of 80 to 300 μm and 400 g of tungsten powder with a particle size of 1 to 5 μm, mix them evenly and put them into a corundum crucible for later use.

[0061] (2) High temperature treatment in vacuum furnace

[0062] The powder in the corundum crucible in step (1) was placed in a vacuum furnace at a temperature of 1050°C and a vacuum degree of 2×10 - 2 After keeping warm for 5 hours under the condition of 1.577 Pa, it is cooled with the furnace.

[0063] (3) Separation of Kovar powder and tungsten powder after plating

[0064] The mixed powder after vacuum high temperature treatment in step (2) is separated by a sieve with a mesh size of 200, and the powder on the sieve is taken to obtain the plated kovar powder.

[0065] (4) Preparation of composite powder

[0066] According to the proportion, take 70g of the plated kovar powder obtained in step (3), and weigh 30g of copper powder with an average particle size of 10μm, and mix them evenly to obtain kovar-copper composite powder.

[0067] (5) Hot pressing sintering

[0068] The Kovar composite powder in step (4) is placed in a graphite mold and sintered on a hot press at a temperature of 900°C, a holding time of 20 minutes, a heating rate of 50°C / min, and a pressure of 50 MPa. After cooling and demolding, the Kovar copper composite material is obtained.

[0069] The performance of the kovarable copper composite material obtained in Example 2 was tested, and the test results are as follows:

[0070] The density of the prepared kovar copper composite material is 8.22 g·cm -3 , density is 98.7%, thermal conductivity is 66.5W·m -1 ·K -1 , thermal expansion coefficient (room temperature to 150°C) is 8.8×10 -6 K -1 .

[0071] Example 2-1, other conditions are the same as Example 2, only the sintering temperature is changed to 800 ° C, the density of the composite material after sintering is 8.18 g cm -3 , density is 98.2%, thermal conductivity is 64.1W·m -1 ·K -1 , thermal expansion coefficient (room temperature to 150°C) is 8.7×10 -6 K -1 .

[0072] Example 2-2, other conditions are the same as Example 2, only the holding time is changed to 30min, the density of the composite material after sintering is 8.25g·cm -3 , density is 99.0%, thermal conductivity is 68.4W·m -1 ·K -1 , thermal expansion coefficient (room temperature to 150°C) is 8.8×10 -6 K -1 .

[0073] Example 2-3, other conditions are the same as Example 2, only the sintering pressure is changed to 30MPa, the density of the composite material after sintering is 8.20g·cm -3 , density is 98.4%, thermal conductivity is 65.2W·m -1 ·K -1 , thermal expansion coefficient (room temperature to 150°C) is 8.7×10 -6 K -1 .

[0074] Example 3

[0075] In this embodiment 3, a fully plated Kovar alloy powder and a Kovar-copper composite material having a fully plated Kovar alloy mass fraction of 80% and a copper mass fraction of 20% are pre-prepared. The preparation process includes the following steps:

[0076] Steps (1) to (3) are the same as those in Example 1.

[0077] (4) Preparation of composite powder

[0078] According to the proportion, take 80g of the plated kovar powder obtained in step (3), and weigh 20g of copper powder with an average particle size of 10μm, and mix them evenly to obtain kovar-copper composite powder.

[0079] (5) Hot pressing sintering

[0080] The Kovar composite powder in step (4) was placed in a graphite mold and sintered on a hot press at a temperature of 950°C, a holding time of 10 min, a heating rate of 40°C / min, and a pressure of 50 MPa. After cooling and demolding, the Kovar copper composite material was obtained.

[0081] The performance of the kovarable copper composite material obtained in Example 3 was tested, and the test results are as follows:

[0082] The density of the prepared kovar copper composite material is 8.13 g·cm -3 , density is 98.5%, thermal conductivity is 55.4W·m -1 ·K -1 , thermal expansion coefficient (room temperature to 150°C) is 8.3×10 -6 K -1 .

[0083] Example 3-1: Other conditions are the same as those in Example 3, except that the sintering temperature is changed to 850°C. The density of the composite material after sintering is 8.09 g·cm -3 , density is 98.1%, thermal conductivity is 53.0W·m -1 ·K -1 , thermal expansion coefficient (room temperature to 150°C) is 8.3×10 -6 K -1 .

[0084] Example 3-2: Other conditions are the same as those in Example 3, except that the holding time is changed to 30 min. The density of the composite material after sintering is 8.18 g·cm -3 , density is 99.2%, thermal conductivity is 58.7W·m -1 ·K -1 , thermal expansion coefficient (room temperature to 150°C) is 8.3×10 -6 K -1 .

[0085] Example 3-3, other conditions are the same as those of Example 3, only the sintering pressure is changed to 30 MPa, and the density of the composite material after sintering is 8.07 g·cm -3 , density is 97.8%, thermal conductivity is 51.9W·m -1 ·K -1 , thermal expansion coefficient (room temperature to 150°C) is 8.3×10 -6 K -1 .

[0086] Comparative Example 1

[0087] In this comparative example 1, the surface of the kovar powder is not plated. The kovar powder and copper powder of the same mass and proportion as those in Example 1 are directly mixed and sintered. The sintering parameters are the same as those in Example 1 to obtain a kovar-copper composite material. The SEM microstructure and element distribution at the interface are shown in the attached figure. Figure 3 As shown. After performance testing, the density of the composite material is 8.36g·cm -3 , density is 98.8%, thermal conductivity is 40.6W·m-1 ·K -1 , thermal expansion coefficient (room temperature to 150°C) is 9.1×10 -6 K -1 .

[0088] Comparative Example 2

[0089] The other conditions are the same as those in Example 1, except that the mixing ratio of kovar powder to tungsten powder is changed to 1:1. The SEM morphology of the kovar powder after plating is shown in the attached figure. Figure 4 The density of the prepared Kovar copper composite material is 8.24 g·cm -3 , thermal conductivity is 55.8W·m -1 ·K -1 , thermal expansion coefficient (room temperature to 150°C) is 9.6×10- 6 K -1 .

[0090] Comparative Example 3

[0091] The other conditions were the same as those in Example 1, except that the vacuum heat treatment temperature after the mixture of kovar powder and tungsten powder was changed to 950°C and 1000°C. The SEM morphology of the kovar powder after plating is shown in the attached figure. Figure 4 b and c. The density of the Kovar copper composite material prepared by using Kovar powder plated at 1000℃ is 8.28g·cm -3 , thermal conductivity is 43.7 W·m -1 ·K -1 , thermal expansion coefficient (room temperature to 150°C) is 9.3×10 -6 K -1 .

[0092] Comparative Example 4

[0093] The other conditions are the same as those in Example 1, except that the vacuum heat treatment temperature of the mixture of kovar powder and tungsten powder is changed to 1150°C. The mixed powder of kovar and tungsten powder after vacuum treatment is sintered into blocks, resulting in the inability to separate the coated kovar powder, and the experiment fails.

[0094] Comparative Example 5

[0095] The other conditions were the same as those in Example 1, except that the vacuum heat treatment time after the mixture of kovar powder and tungsten powder was changed to 2 h. The SEM morphology of the kovar powder after plating is shown in the attached figure. Figure 4 d. The density of the prepared Kovar copper composite material is 8.21 g·cm -3 , thermal conductivity is 48.6W·m -1 ·K -1 , thermal expansion coefficient (room temperature to 150°C) is 9.6×10 -6 K -1。

Claims

1. A surface modified kovar powder reinforced copper-based composite material, characterized in that: The surface modified Kovar powder reinforced copper-based composite material comprises a Kovar alloy, a coating layer and copper. The coating layer is coated on the Kovar alloy. The Kovar alloy coated with the coating layer is uniformly distributed in the copper. The coating layer is a tungsten-containing coating layer.

2. A method for preparing the surface-modified kovar powder reinforced copper-based composite material according to claim 1, characterized in that: First, tungsten powder and kovar powder are mixed and then subjected to vacuum high-temperature treatment. The kovar powder and tungsten powder after high-temperature treatment are separated to obtain a completely coated kovar powder, which is then mixed with copper powder and hot-pressed and sintered to obtain a surface-modified kovar powder-reinforced copper-based composite material.

3. The method for preparing a surface-modified kovar powder reinforced copper-based composite material according to claim 2, characterized in that: The following steps are involved: Step 1: According to the mass ratio of tungsten powder to kovar alloy powder = 3-5, weigh tungsten powder and kovar alloy powder and mix them thoroughly; the particle size of the tungsten powder used is less than or equal to 0.1d; the d is the particle size of the kovar alloy powder; Step 2: Place the mixed powder in a vacuum furnace for high temperature treatment; the high temperature treatment temperature is 1050°C to 1100°C; the heat preservation time is 2 to 5 hours; Step 3: Separating the tungsten / Kovar mixed powder after high temperature treatment to obtain Kovar alloy powder with a coating layer; Step 4: weigh the Kovar alloy powder with a coating layer and the copper powder and mix them thoroughly according to the mass ratio of Kovar alloy powder with a coating layer: copper powder = 40-80:60-20; obtain Kovar-copper composite powder; Step 5: Load the Kovar-copper composite powder into a mold and perform vacuum hot pressing and sintering to obtain a surface-modified Kovar powder-reinforced copper-based composite material.

4. The method for preparing a surface-modified kovar powder reinforced copper-based composite material according to claim 3, characterized in that: The mass ratio of the tungsten powder to the kovar powder in step 1 is 3 to 5, preferably 4 to 5.

5. The method for preparing a surface-modified kovar powder reinforced copper-based composite material according to claim 3, characterized in that: The particle size of the kovar powder described in step 1 is 80-300 μm, and the particle size of the tungsten powder is 1-5 μm.

6. The method for preparing a surface-modified kovar powder reinforced copper-based composite material according to claim 3, characterized in that: The conditions of the vacuum high temperature treatment in step 2 are: insulation temperature 1050°C to 1100°C; insulation time 2 to 5 hours, preferably 4 to 5 hours; vacuum degree 9×10 -3 ~2×10 -2 Pa; cooling with the furnace.

7. The method for preparing a surface-modified kovar powder reinforced copper-based composite material according to claim 3, characterized in that: In step 3, the tungsten / Kovar mixed powder after high temperature treatment is separated by sieve to obtain Kovar alloy powder with complete coating; the mesh number of the sieve used is 200 mesh; The complete coating of the Kovar alloy powder described in step 3 is a tungsten-iron compound.

8. The method for preparing a surface-modified kovar powder reinforced copper-based composite material according to claim 3, characterized in that: In the kovar copper composite powder described in step 4, the mass percentage of the kovar alloy powder with the coating layer is 40% to 80%.

9. The method for preparing a surface-modified kovar powder reinforced copper-based composite material according to claim 3, characterized in that: The hot pressing sintering conditions described in step 5 are: temperature of 750-950° C., preferably 800-950° C., more preferably 800-910° C.; holding time of 10-30 min, preferably 20-30 min; heating rate of 30-50° C. / min; pressure of 30-50 MPa; In step five, the mold used is preferably a carbon mold, and more preferably a graphite mold.

10. The method for preparing a surface-modified kovar powder reinforced copper-based composite material according to claim 3, characterized in that: When the mass ratio of the kovar alloy with the coating layer to copper is 6:4, the density of the obtained kovar-copper composite material is 8.31-8.35 g·cm -3 , density is greater than or equal to 99%, thermal conductivity is 85~86W·m -1 ·K -1 The thermal expansion coefficient from room temperature to 150°C is (9.6~9.8)×10 -6 K -1 ; When the mass ratio of the kovar alloy with the coating layer to copper is 7:3, the density of the obtained kovar-copper composite material is 8.2-8.25 g·cm -3 , density is greater than or equal to 98.5%, thermal conductivity is 66~67W·m -1 ·K -1 The thermal expansion coefficient from room temperature to 150°C is (8.7~8.9)×10 -6 K -1 ; When the mass ratio of the kovar alloy with the coating layer to copper is 8:2, the density of the obtained kovar-copper composite material is 8.1-8.15 g·cm -3 , density is greater than or equal to 98.5%, thermal conductivity is 55~55.6W·m -1 ·K -1 The thermal expansion coefficient from room temperature to 150°C is (8.2~8.4)×10 -6 K -1 .