Preparation process of low-titanium high-purity silicon iron

By using low-titanium silicate, fruit shell carbonization material and orchid as raw materials, combined with electric heating and external oxygen refining technology, the problems of high titanium content and petroleum coke pollution in smelting high-purity ferrosilicon are solved, and low titanium is achieved The preparation of high-purity ferrosilicon reduces energy consumption and environmental pollution and improves product quality.

CN118910494APending Publication Date: 2024-11-08SHIZUISHAN CITY HUINONG DISTRICT HONGFENG IND &TRADE CO
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411010126.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The prior art has a high titanium content when smelting high-purity ferrosilicon, which affects the fatigue life of silicon steel, and the environmental pollution and high energy consumption problems caused by petroleum coke have not been effectively solved.

Method used

Low-titanium silicate, fruit shell carbonization material and low-titanium orchid carbon as raw materials, and using electric heating and external oxygen blowing refining technology, replacing petroleum coke through fruit shell carbonization material, reducing titanium content, and blowing air and oxygen outside the furnace Refine to reduce trace elements residues.

Benefits of technology

The preparation of low-titanium high-purity ferrosilicon with Ti≤0.01% was achieved, which reduced energy consumption and environmental pollution, improved product quality and output, and avoided the safety hazards of traditional chlorination refining methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910494A_ABST
    Figure CN118910494A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation process of low-titanium high-purity silicon iron. The preparation process specifically comprises the following steps: S1, burdening: preparing silica, semi-coke, a shell carbonized material and a silicon steel sheet according to the ratio of a formula, crushing and uniformly mixing to obtain a furnace charge; s2, smelting: uniformly feeding furnace charge into the furnace, preheating, melting and reacting the furnace charge in the furnace under the condition of electric heating to form silicon molten iron, and feeding the silicon molten iron into a furnace bottom molten pool; s3, discharging: when the molten iron at the bottom of the furnace is accumulated to a certain amount, opening an iron outlet, and enabling the molten iron to flow into a ladle; s4, an air brick core is added to the bottom of the ladle, air is introduced, and meanwhile a slag agent is added for external refining; s5, casting, crushing and packaging are conducted after refining is completed, and the high-purity ferrosilicon is obtained.The method has the beneficial effects that the shell carbonized material is adopted as a reducing agent, and the content of the titanium element in the high-purity ferrosilicon can be reduced to the maximum extent; and meanwhile, potential safety hazards and environmental protection problems existing in a chlorination refining method are effectively solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ferrosilicon preparation, in particular to a preparation process of low-titanium high-purity ferrosilicon. Background Art

[0002] High-grade silicon steel is an essential soft magnetic alloy used in the power, electronics, and military industries, primarily used as the cores of various motors, generators, and transformers. Low-titanium, high-purity ferrosilicon is an essential alloying additive and deoxidizer for the smelting of high-grade grain-oriented silicon steel. Titanium is a harmful element with a strong affinity for nitrogen dissolved in steel, often remaining in the steel as titanium nitride and titanium carbonitride inclusions, severely impacting the steel's fatigue life. The harmful effects of titanium inclusions are particularly pronounced when other oxide inclusions are present in small quantities. Therefore, with the development of high-grade silicon steel, the demand for higher titanium content in high-purity ferrosilicon is increasing.

[0003] Currently, high-purity ferrosilicon is produced both domestically and internationally by reducing silica, metallurgical coke (petroleum coke, charcoal, blue carbon, etc.), and steel scrap (or iron ore) in a submerged arc furnace. This method produces ferrosilicon with high levels of trace elements such as titanium, which does not meet the requirements for producing high-grade silicon steel. Furthermore, the high sulfur content of petroleum coke, used as a reducing agent, poses a significant environmental risk. Furthermore, charcoal, with its high ash content and high moisture content, also has relatively low reactivity, resulting in high energy consumption during the production of high-purity ferrosilicon. Therefore, a new production process has been proposed. Summary of the Invention

[0004] The purpose of the present invention is to provide a preparation process of low-titanium high-purity ferrosilicon to solve the problems raised in the above background technology.

[0005] To achieve the above object, the present invention provides the following technical solutions:

[0006] A preparation process for low-titanium high-purity ferrosilicon, specifically comprising the following steps:

[0007] S1. Batching: Prepare, crush and evenly mix silica, semi-coke, carbonized fruit shell material and silicon steel sheet according to the ratio of the formula to obtain furnace charge;

[0008] S2. Melting: The charge is evenly fed into the furnace. Under the condition of electric heating, the charge in the furnace is preheated, melted, and reacted to form ferrosilicon liquid which enters the molten pool at the bottom of the furnace;

[0009] S3. Tapping: When the molten iron at the bottom of the furnace accumulates to a certain amount, the taphole is opened to allow the molten iron to flow into the ladle;

[0010] S4. Add a breathable brick core at the bottom of the ladle to allow air to pass through, and add slag agent for refining outside the furnace;

[0011] S5. After refining, it is cast, crushed and packaged to obtain high-purity ferrosilicon.

[0012] As a preferred solution of the present invention: the ratio of the silica, semi-coke, fruit shell carbonized material and silicon steel sheet is 1:0.3-0.35:0.2-0.25:0.1-0.2.

[0013] As a preferred solution of the present invention: a bag dust collector is used to remove dust during the crushing and mixing processes of the mixed raw materials in S1.

[0014] As a preferred embodiment of the present invention, the steps for processing the silicon powder produced in S2 are as follows:

[0015] S2.1. Use air cooler to cool the slag;

[0016] S2.2, perform preliminary dust collection using a dust collector and fan;

[0017] S2.3. Collect the dust again using a bag vacuum cleaner to obtain microsilica powder.

[0018] As a preferred solution of the present invention: in said S3, the molten iron at the bottom of the furnace accumulates and submerges the taphole, and the taphole is opened when the liquid level is 5-10 cm higher than the taphole.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] 1. Optimize the raw material formula of low-titanium high-purity ferrosilicon: Use low-titanium silicate, fruit shell carbonized material, low-titanium blue carbon, and silicon steel sheets as raw materials to develop low-titanium high-purity ferrosilicon with Ti≤0.01%, which is used to produce special silicon steel. Use fruit shell carbonized material instead of petroleum coke as a reducing agent. Utilize the characteristics of fruit shell carbonized material such as high fixed carbon, low ash content, and good reaction activity to ensure high product quality and increase product output. In the production process, the energy consumption of 10,000 yuan of output value of low-titanium high-purity ferrosilicon can be greatly reduced.

[0021] 2. Off-furnace oxygen blowing refining technology: By blowing air and oxygen into the molten iron ladle and adding slag agent, trace elements such as calcium, aluminum, carbon, and manganese in the ferrosilicon molten iron are removed, replacing the traditional chlorination refining method, effectively reducing the pollution of toxic gas chlorine to the environment and the safety hazards in the production process. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION

[0023] The following will clearly and completely describe the technical solutions in the embodiments of the present invention in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of the present invention.

[0024] Example 1

[0025] See also Figure 1 , a preparation process of low-titanium high-purity ferrosilicon, specifically comprising the following steps:

[0026] S1. Batching: Silica, semi-coke, carbonized fruit shell material, and silicon steel sheet are crushed and evenly mixed in a ratio of 1:0.35:0.25:0.2 to obtain furnace charge. During the entire crushing and mixing process, a bag dust collector is used for dust removal.

[0027] S2. Melting: The charge is evenly fed into the furnace. Under the condition of electric heating, the charge in the furnace is preheated, melted, and reacted to form ferrosilicon liquid which enters the molten pool at the bottom of the furnace;

[0028] S3. Tapping: When the molten iron at the bottom of the furnace submerges the tapping hole, open the tapping hole when the liquid level is 5 cm above the tapping hole to allow the molten iron to flow into the ladle.

[0029] S4. Add a breathable brick core at the bottom of the ladle to allow air to pass through, and add slag agent for refining outside the furnace;

[0030] S5. After refining, it is cast, crushed and packaged to obtain high-purity ferrosilicon.

[0031] Example 2

[0032] See also Figure 1 , the remaining slag treatment steps in S2 are as follows:

[0033] S2.1. Use air cooler to cool the slag;

[0034] S2.2, perform preliminary dust collection using a dust collector and fan;

[0035] S2.3. Collect the dust again using a bag vacuum cleaner to obtain microsilica powder.

[0036] Specifically, the complete process of this process is:

[0037] The first step is to crush and evenly mix silica, semi-coke, carbonized fruit shell material, and silicon steel sheet in a ratio of 1:0.35:0.25:0.2 to obtain furnace charge. During the entire crushing and mixing process, a bag dust collector is used for dust removal.

[0038] The second step is to evenly feed the charge into the furnace. Under the condition of electric heating, the charge in the furnace is preheated, melted, and reacted to form ferrosilicon water which enters the molten pool at the bottom of the furnace.

[0039] The third step is to open the taphole when the molten iron at the bottom of the furnace submerges the taphole and the liquid level is 5 cm higher than the taphole to allow the molten iron to flow into the ladle. After the molten iron has flowed out, an air cooler is connected to cool the slag, and the dust is collected by a bag vacuum cleaner to obtain microsilica powder.

[0040] Step 4: Add a breathable brick core at the bottom of the ladle to allow air to pass through, and add slag agent for refining outside the furnace;

[0041] Step 5: After refining, it is cast, crushed and packaged to obtain high-purity ferrosilicon.

[0042] While embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions, and variations may be made to these embodiments without departing from the principles and spirit of the invention, and that the scope of the invention is defined by the appended claims and their equivalents.

Claims

1. A process for preparing low-titanium high-purity ferrosilicon. It is characterized in that The specific steps include: S1. Batching: Prepare, crush and evenly mix silica, blue charcoal, fruit shell carbonized material and silicon steel sheet according to the ratio of the formula to obtain the furnace charge; S2. Melting: The charge is evenly fed into the furnace. Under the condition of electric heating, the charge in the furnace is preheated, melted, and reacted to form ferrosilicon water which enters the molten pool at the bottom of the furnace; S3, tapping: When the molten iron at the bottom of the furnace accumulates to a certain amount, the tapping hole is opened to allow the molten iron to flow into the ladle; S4. Add a permeable brick core at the bottom of the ladle to ventilate the air, and add slag agent for refining outside the furnace; S5. After refining, it is cast, crushed and packaged to obtain high-purity ferrosilicon.

2. A process for preparing low-titanium high-purity ferrosilicon according to claim 1, Features: The ratio of silica, semi-coke, carbonized fruit shell material and silicon steel sheet is 1:0.3-0.35:0.2-0.25:0.1-0.

2.

3. A process for preparing low-titanium high-purity ferrosilicon according to claim 1, Features: A bag dust collector is used to remove dust during the crushing and mixing of the mixed raw materials in S1.

4. A process for preparing low-titanium high-purity ferrosilicon according to claim 1, Features: The steps for processing the silicon powder produced in S2 are as follows: S2.

1. Use an air cooler to cool the slag; S2.2, preliminary dust collection by dust collector and fan; S2.

3. Collect the dust again through a bag vacuum cleaner to obtain microsilica powder.

5. A process for preparing low-titanium high-purity ferrosilicon according to claim 1, Features: In the S3, the molten iron at the bottom of the furnace accumulates and submerges the tapping hole, and the tapping hole is opened when the liquid level is 5-10 cm higher than the tapping hole.