500MPa-grade atmospheric corrosion resistant steel bar and production method thereof
By reasonably formulating elements such as C, Si, Mn, Cu, V in the steel bars and using specific metallurgical processes to form ferrite and pearlite tissues, traditional atmospheric corrosion-resistant steel bars have high prices, narrow usage range and production efficiency. The problem of low efficiency and low cost 500MPa grade atmospheric corrosion-resistant steel bars has been achieved, improving its strength and corrosion resistance.
Patent Information
- Application Number
- CN202411040837.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-08
AI Technical Summary
Traditional atmospheric corrosion-resistant steel bars are expensive, have limited use range, have long production process time, harsh conditions, low production efficiency, and are difficult to promote on a large scale.
The chemical components of 500MPa-level atmospheric corrosion-resistant steel bars include C, Si, Mn, Cu, V and other elements. Through the initial refining of converter, LF refining, billet continuous casting and rolling processes, the alloy composition and process parameters are controlled to form ferrite. The microstructure of the body and pearlite improves the strength and corrosion resistance of the steel bars.
The use of alloy elements is reduced, the yield strength, tensile strength and corrosion resistance of the steel bars are improved, the production process is optimized, the production efficiency is improved, and good strength and corrosion resistance are obtained.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of iron and steel metallurgy, and specifically relates to a 500MPa-grade atmospheric corrosion-resistant steel bar and a production method thereof. Background Art
[0002] The rapid development of construction in various regions of my country has increased the demand for construction steel. At the same time, people have higher requirements on the safety and service life of buildings. Therefore, construction steel bars are required to have not only good seismic resistance but also good corrosion resistance.
[0003] In recent years, relevant research has been accelerated in China. Traditional atmospheric corrosion-resistant steel bars are added with alloys such as Cu, Cr and Mo to improve corrosion resistance. However, the alloy element content is too high, the price is high and the scope of use is limited. At the same time, due to the large amount of alloy added, the process of high-temperature and long-term heating + high-temperature rolling + non-water cooling is required, the production efficiency is low, and it is difficult to promote and use on a large scale. Summary of the invention
[0004] The purpose of the present invention is to provide a 500MPa grade atmospheric corrosion resistant steel bar and a production method thereof, so as to solve the problems that conventional atmospheric corrosion resistant steel bars are expensive, have a limited scope of use, have a long production process, harsh conditions and low production efficiency.
[0005] In order to achieve the above object, the present invention adopts the following technical scheme: A 500MPa grade atmospheric corrosion resistant steel bar, the chemical composition of which, by mass percentage, comprises: C: 0.18-0.21%, Si: 0.5-0.6%, Mn: 1.3-1.4%, Cu: 0.25-0.45%, P: 0.05-0.07%, S: 0.008-0.01%, V: 0.05-0.08%, Ti≤0.1%, Al≤0.1%, the balance being Fe and inevitable impurities, the microstructure of the steel bar being ferrite and pearlite, the grain size of the steel bar being grade 9-10, the yield strength of the steel bar being 515-550MPa, the tensile strength being 670-710MPa, and the total elongation under maximum force being 12-14.5%.
[0006] C plays a role in solution strengthening and carbide precipitation strengthening; however, the higher the C content, the lower the weldability and corrosion resistance of the steel. The C content of the steel bars of the present invention is significantly lower than that of the existing steel bars (0.22 - 0.28%), while ensuring the comprehensive mechanical properties of the steel and saving the addition amount of alloys; Si undergoes solution strengthening to increase the strength of the steel and obtain a low yield ratio, but too high a content will significantly reduce the plasticity and toughness of the steel; Mn is a deoxidizer and desulfurizer, which plays a role in solution strengthening to increase the strength of the steel and helps to improve the stability of austenite in the steel; if the Mn content is too high, segregation will occur during casting, affecting the stability of the microstructure and thus the mechanical properties, resulting in poor cold bending performance of the steel bars; V has the effects of precipitation strengthening and grain refinement strengthening, can simultaneously increase the strength and toughness of the steel, ensure the elongation performance of the steel, and at the same time V also has the effect of refining grains, playing a role in pinning the austenite grain boundaries and inhibiting the growth of austenite; Cu is an element that effectively improves the atmospheric corrosion resistance, can densify the rust layer, prevent the transmission of air and moisture into the steel matrix, increase the self-corrosion potential of the steel matrix and promote the passivation of the steel matrix.
[0007] The production method of the above 500 MPa grade atmospheric corrosion resistant steel bars includes the following steps: S1: KR desulfurization of hot metal: The conditions of the hot metal entering the furnace are controlled as follows, Si: 0.30 - 0.50%, P: ≤0.20%, S: ≤0.30%, temperature ≥1250 °C. After the blast furnace hot metal arrives at the steelmaking workshop, CaO powder is sprayed into the hot metal ladle to promote the formation of CaS from S in the hot metal, and then the CaS slag is removed through slag skimming equipment; S2: Primary refining in the converter: High-quality scrap steel is used to reduce the mixing of impurities, and the copper plate is added to the furnace with the scrap steel at the lower limit; During the converter blowing process, high-pulling and supplementary blowing are used to control the lance position and control the process splash; Slag materials are added during the converter blowing process, and the addition amount of each batch of slag materials ≤500 Kg, and the slag materials must be added within 3 minutes before the end point to achieve early slag melting in the initial stage and thorough slag melting in the process; The basicity of the final slag is controlled at R = 2.8 - 3.2, and the lance lowering time at the end point >30 s; Bottom blowing nitrogen stirring is used in the early stage of the converter blowing process, and pure argon stirring is switched to in the middle and later stages; End point control: 0.04% < C < 0.05%, and strong bottom blowing stirring is carried out at the end of blowing, with the flow rate controlled at 200 M 3The above ensures that the final molten steel is not oxidized under the condition of low carbon; the tapping temperature of the converter is controlled between 1610℃ and 1630℃, and the final temperature can be increased by 10-30℃ according to the ladle condition and abnormal conditions; use a ladle with good air permeability and clean turnover, open bottom nitrogen or argon 1-2 minutes before tapping, stir with a large amount of air during the tapping process to ensure that the alloy is fully melted, ensure red envelope tapping, and the ladle baking temperature is >900℃; slag blocking tapping to prevent large amounts of slag, and the slag layer thickness in the ladle is <50mm; deoxidation and alloying: when one-quarter of the steel is discharged, add silicon manganese, composite deoxidizer, phosphorus iron, and vanadium nitrogen alloy in turn, and add them when three-quarters of the molten steel is discharged; tapping slag washing: slag washing material is added with the steel flow during the tapping process, and the addition amount is 1~3 kg / t steel, adding time is one quarter of the steel, together with the alloy; argon is blown at the bottom of the steel tapping process, and the stirring intensity is controlled during the stirring process. The exposed diameter of molten steel on the ladle surface reaches 500mm, and at the same time, the temperature before argon is ensured to be met; the ladle is blown in the argon station for 3 minutes to take samples, and argon is blown for 5 minutes after the composition is adjusted; S3: LF refining: When the ladle arrives at the refining site, the temperature is measured immediately and argon is passed. The argon pressure and flow rate are suitable for slightly turning the slag surface without exposing the molten steel. Lime + composite refining slag is used for slag making. During the refining process, the refining submerged arc operation is ensured to control the refining slag, quickly turn the slag into white slag, and perform soft argon blowing; S4: Billet continuous casting: control the superheat to 15-35℃; use magnesium dry material for the working layer of the tundish, and the baking temperature is ≥1000℃; use a long nozzle from the large ladle to the tundish and a sealing cover for the tundish to reduce temperature drop and secondary oxidation; use an aluminum-carbon immersion nozzle from the tundish to the crystallizer to ensure verticality and centering, and the insertion depth of the immersion nozzle is 90±10 mm; use a special protective slag for acid-resistant steel for the crystallizer protective slag, which must be dry and black-faced, and electromagnetic stirring is used during the production process; continuous casting cooling, the temperature before straightening is ≥900℃; ensure that the nozzle is not blocked, the water spray is uniform, and the position is centered to ensure the quality of the steel billet, and the surface is inspected and cleaned; S5: Heating: The temperature of the preheating section is ≤980℃. The heating temperature of the heating section and the soaking section is increased in the heating furnace. The furnace time is ≥120min to ensure that the alloy elements V, Cu, etc. are fully and evenly dissolved in the austenite matrix. S6: Rolling: In the rolling process, micro-pile or micro-drawing rolling is adopted for rough rolling and intermediate rolling, and loop tension-free rolling is adopted for finishing rolling to avoid drawing steel rolling. Air cooling process is adopted after rolling to improve the strength of steel without sacrificing toughness, promote grain refinement, increase the yield strength and tensile strength of the material, improve the uniformity of the organization, and help to obtain a more uniform microstructure.
[0008] Preferably, the slag material in step S2 includes lime, dolomite and temperature regulating material, with lime accounting for 2 / 3 of the first batch, 1 / 3 of the later batch, all of the dolomite, 3 / 4 of the temperature regulating material being added, and the rest being adjusted during "re-drying".
[0009] Preferably, the soft argon blowing time in step S3 shall not be less than 8 minutes.
[0010] Preferably, the middle package in step S4 is a stopper package or a sizing quick-change package.
[0011] Preferably, the continuous casting cooling in step S4 adopts a slow cooling mode, which reduces the amount of cooling water by 10% compared with conventional cooling water.
[0012] Preferably, in step S5, the temperature of the heating section is controlled at 1150°C to 1200°C.
[0013] Preferably, in step S6, the starting rolling temperature of rough rolling is 1120°C to 1140°C, the starting rolling temperature of finishing rolling is 990°C to 1030°C, the final rolling temperature of finishing rolling is 1000°C to 1040°C, and the temperature of the upper cooling bed for air cooling is 990°C to 1000°C.
[0014] Preferably, in step S6, pre-watering treatment is performed during the rolling process, no watering is performed after rolling, and the cooling rate of air cooling after rolling is controlled at 1-2°C / s.
[0015] Compared with the prior art, the present invention has the following beneficial effects: The production method of the present invention controls the contents of alloy elements C, Si, Mn, Cu, V, P and S in the primary refining of the converter to ensure the uniformity of the alloy components, reduce the alloy endothermic temperature drop in the steel-making process, optimize the alloy component system of elements such as Cu and V, optimize the smelting process, refine the grains of the steel, improve the strength index of the steel bar, adopt the process of "water penetration during the process + slow cooling after rolling", reasonably control the heating temperature, the start rolling temperature of the rough refining, the finishing rolling temperature and the upper cooling bed temperature, adopt a slow cooling cooling method, make the steel bar structure ferrite and pearlite, and the obtained steel bar has good strength and toughness and corrosion resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 This is the microstructure diagram of the φ25mm atmospheric corrosion resistant steel bar of Example 1; Figure 2 This is the microstructure diagram of the φ14 mm atmospheric corrosion resistant steel bar of Example 3; Figure 3 The atmospheric corrosion resistant steel bars of φ25 mm in Example 1 and Example 2 and the ordinary steel bars are mixed at a concentration of 1.0 × 10 -2 The corrosion external morphology of the corrosion sample after immersion in mol / L NaHSO3 solution for 72 hours; Figure 4 The atmospheric corrosion resistant steel bars of φ14 mm in Example 3 and Example 4 and the ordinary steel bars are mixed at a concentration of 1.0 × 10 -2 mol / L NaHSO3 The corrosion external morphology of the corrosion sample after immersion in the solution for 72 hours. DETAILED DESCRIPTION
[0017] The embodiments of the present invention are further described below in conjunction with the accompanying drawings and embodiments. Example 1
[0018] A method for producing 500MPa grade atmospheric corrosion resistant steel bars comprises the following steps: S1: Hot metal KR desulfurization: The hot metal conditions entering the furnace are controlled as follows: Si: 0.30%, P: 0.20%, S: 0.30%, temperature 1250℃. After the hot metal from the blast furnace arrives at the steelmaking workshop, CaO powder is sprayed into the hot metal ladle to promote the S in the hot metal to react with CaO to generate CaS, and then the CaS slag is removed by the slag removal equipment; S2: Converter primary refining: Use high-quality scrap steel to reduce impurities, and add copper plates into the furnace with scrap steel according to the lower limit; use high-pull supplementary blowing to control the gun position and control process splashing during converter refining; add lime, dolomite and temperature regulating materials during converter refining, according to the first batch of lime 2 / 3, the later 1 / 3, all dolomite, and 3 / 4 temperature regulating materials. The amount of slag added to each batch is 500Kg, and the slag must be added 3 minutes before the end point to achieve early slag in the early stage and thorough slag in the process; the final slag basicity is controlled at R=2.9, and the end point gun pressure time is 40 s; bottom blowing nitrogen stirring is used in the early stage of converter refining, and pure argon stirring is switched in the middle and late stages; end point control: C is 0.045%, bottom blowing strong stirring is carried out at the end of refining, and the flow rate is controlled at 200M 3 The above ensures that the final molten steel does not oxidize under the condition of low carbon; the converter tapping temperature is controlled between 1610℃ and 1630℃, and the final temperature can be increased by 10-30℃ according to the ladle condition and abnormal conditions; use a ladle with good air permeability and clean turnover, open bottom nitrogen blowing 2 minutes before tapping, stir with a large amount of air during tapping to ensure that the alloy is fully melted, ensure red envelope tapping, and the ladle baking temperature is 920℃; slag blocking tapping to prevent large amounts of slag, the slag layer thickness in the ladle is <50mm; deoxidation and alloying: when one quarter of the steel is discharged, add silicon manganese, composite deoxidizer, phosphorus iron, and vanadium nitrogen alloy in turn, and add them when the molten steel is discharged to three quarters; tapping slag washing: slag washing material is added with the steel flow during the tapping process, and the addition amount is 1.5 kg / t steel, adding time is one quarter of the steel, together with the alloy; argon is blown at the bottom of the steel tapping process, and the stirring intensity is controlled during the stirring process. The exposed diameter of molten steel on the ladle surface reaches 500mm, and at the same time, the temperature before argon is ensured to be met; the ladle is blown in the argon station for 3 minutes to take samples, and argon is blown for 5 minutes after the composition is adjusted; S3: LF refining: When the ladle arrives at the refining site, the temperature is measured immediately and argon is passed. The argon pressure and flow rate are suitable for slightly turning the slag surface without exposing the molten steel. Lime + composite refining slag is used for slag making. During the refining process, the refining submerged arc operation is ensured to control the refining slag, quickly turning the slag into white slag, and soft argon blowing is carried out. The soft argon blowing time is 9 minutes; S4: Billet continuous casting: control the superheat at 20℃; magnesium dry material is used in the working layer of the tundish, and the baking temperature is 1000℃; long nozzles are used from the large ladle to the tundish and sealing covers are used in the tundish to reduce temperature drop and secondary oxidation; aluminum carbon immersion nozzles are used from the tundish to the crystallizer to ensure verticality and centering, and the insertion depth of the immersion nozzle is 95 mm; the crystallizer protective slag uses acid-resistant steel special protective slag, which must be dry, black surface operation, electromagnetic stirring is used in the production process, the current is 150A, and the frequency is 3Hz; continuous casting cooling, the temperature before straightening is 900℃; ensure that the nozzle is not blocked, the water spray is uniform, and the position is centered to ensure the quality of the steel billet, and the surface is inspected and cleaned; S5: Heating: The preheating temperature is 980°C, and the heating temperature of the heating section is increased in the heating furnace to 1160°C. The furnace time is 120 minutes to ensure that the alloy elements V, Cu, etc. are fully and evenly dissolved in the austenite matrix; S6: Rolling: During the rolling process, micro-pile or micro-drawing rolling is adopted for rough rolling and intermediate rolling. The starting rolling temperature of rough rolling is 1060℃, and the finishing rolling adopts loop tension-free rolling to avoid steel drawing rolling. The starting rolling temperature of finishing rolling is 1000℃, and the final rolling temperature of finishing rolling is 1010℃. After rolling, air cooling process is adopted, and the cooling rate is controlled at 2℃ / s. Pre-water penetration treatment is carried out during the rolling process, and no water penetration is carried out after rolling. The strength of steel is improved without sacrificing toughness, grain refinement is promoted, the yield strength and tensile strength of the material are improved, and the uniformity of the organization is improved, which helps to obtain a more uniform microstructure.
[0019] The 500MPa grade atmospheric corrosion resistant steel bar obtained by the production method has the following chemical compositions by mass percentage: C: 0.18%, Si: 0.6%, Mn: 1.4%, Cu: 0.4%, P: 0.06%, S: 0.009%, V: 0.07%, Ti: 0.09%, Al: 0.08%, and the balance is Fe and unavoidable impurities.
[0020] The yield strength of the φ25mm steel bar obtained by this production method is 525MPa, the tensile strength is 690MPa, and the total elongation under maximum force is 14.2%. Figure 1 As shown in Figure 1, the microstructure of the steel bar is ferrite and pearlite, and the grain size of the steel bar is level 9. Figure 3 As shown in the 72-hour immersion accelerated corrosion test, the average corrosion rate is 3.3245 g / (m 2 ·h), the relative corrosion rate is 54.5%. Example 2
[0021] A method for producing 500MPa grade atmospheric corrosion resistant steel bars comprises the following steps: S1: Hot metal KR desulfurization: The hot metal conditions entering the furnace are controlled as follows: Si: 0.30%, P: 0.20%, S: 0.30%, temperature 1280℃. After the hot metal from the blast furnace arrives at the steelmaking workshop, CaO powder is sprayed into the hot metal ladle to promote the S in the hot metal to react with CaO to generate CaS, and then the CaS slag is removed by the slag removal equipment; S2: Converter primary refining: Use high-quality scrap steel to reduce impurities, and add copper plates into the furnace with scrap steel according to the lower limit; use high-pull supplementary blowing to control the gun position and control process splashing during converter refining; add lime, dolomite and temperature regulating materials during converter refining, according to the first batch of lime 2 / 3, the later 1 / 3, all dolomite, and 3 / 4 temperature regulating materials. The amount of slag added to each batch is 490Kg, and the slag must be added 3 minutes before the end point to achieve early slag in the early stage and thorough slag in the process; the final slag basicity is controlled at R=3.0, and the end point gun pressure time is 35 s; bottom blowing nitrogen stirring is used in the early stage of converter refining, and pure argon stirring is switched in the middle and late stages; end point control: C is 0.042%, bottom blowing strong stirring is carried out at the end of refining, and the flow rate is controlled at 200M 3 The above ensures that the final molten steel is not oxidized under the condition of low carbon; the tapping temperature of the converter is controlled between 1610℃ and 1630℃, and the final temperature can be increased by 10-30℃ according to the ladle condition and abnormal conditions; use a ladle with good air permeability and clean turnover, open the bottom argon gas 1.5min in advance before tapping, stir with a large amount of air during the tapping process to ensure that the alloy is fully melted, ensure red envelope tapping, and the ladle baking temperature is 910℃; slag blocking tapping, prevent large amounts of slag, and the slag layer thickness in the ladle is <50mm; deoxidation and alloying: when one quarter of the steel is discharged, add silicon manganese, composite deoxidizer, phosphorus iron, and vanadium nitrogen alloy in turn, and add them when the molten steel is discharged to three quarters; tapping slag washing: slag washing material is added with the steel flow during the tapping process, and the addition amount is 2 kg / t steel, adding time is one quarter of the steel, together with the alloy; argon is blown at the bottom of the steel tapping process, and the stirring intensity is controlled during the stirring process. The exposed diameter of molten steel on the ladle surface reaches 500mm, and at the same time, the temperature before argon is ensured to be met; the ladle is blown in the argon station for 3 minutes to take samples, and argon is blown for 5 minutes after the composition is adjusted; S3: LF refining: When the ladle arrives at the refining site, the temperature is measured immediately and argon is passed. The argon pressure and flow rate are suitable for slightly turning the slag surface without exposing the molten steel. Lime + composite refining slag is used for slag making. During the refining process, the refining submerged arc operation is ensured to control the refining slag, quickly turning the slag into white slag, and soft argon blowing is carried out. The soft argon blowing time is 10 minutes; S4: Billet continuous casting: control the superheat at 18℃; magnesium dry material is used in the working layer of the tundish, plug rod package or sizing quick-change package is used, and the baking temperature is 1000℃; long nozzles are used from the large ladle to the tundish and sealing covers are used for the tundish to reduce temperature drop and secondary oxidation; aluminum carbon immersion nozzles are used from the tundish to the crystallizer to ensure verticality and centering, and the insertion depth of the immersion nozzle is 85mm; the crystallizer protective slag uses acid-resistant steel special protective slag, the protective slag must be dry, black surface operation, electromagnetic stirring is used in the production process, the current is 150A, and the frequency is 3Hz; continuous casting cooling, the temperature before straightening is 910℃; ensure that the nozzle is not blocked, the water spray is uniform, and the position is centered to ensure the quality of the steel billet, and the surface is inspected and cleaned; S5: Heating: The preheating temperature is 990°C, and the heating temperature of the heating section is increased in the heating furnace to 1165°C. The furnace time is 130 minutes to ensure that the alloy elements V, Cu, etc. are fully and evenly dissolved in the austenite matrix; S6: Rolling: During the rolling process, micro-pile or micro-drawing rolling is adopted for rough rolling and intermediate rolling. The starting rolling temperature of rough rolling is 1060℃, and the finishing rolling adopts loop tension-free rolling to avoid steel drawing rolling. The starting rolling temperature of finishing rolling is 1005℃, and the final rolling temperature of finishing rolling is 1020℃. After rolling, air cooling process is adopted, and the cooling rate is controlled at 2℃ / s. Pre-water penetration treatment is carried out during the rolling process, and no water penetration is carried out after rolling. The strength of steel is improved without sacrificing toughness, grain refinement is promoted, the yield strength and tensile strength of the material are improved, and the uniformity of the organization is improved, which helps to obtain a more uniform microstructure.
[0022] The 500MPa grade atmospheric corrosion resistant steel bar obtained by the production method has the following chemical compositions by mass percentage: C: 0.19%, Si: 0.55%, Mn: 1.3%, Cu: 0.35%, P: 0.05%, S: 0.008%, V: 0.06%, Ti: 0.1%, Al: 0.09%, and the balance is Fe and unavoidable impurities.
[0023] The yield strength of the φ25mm steel bar obtained by this production method is 545MPa, the tensile strength is 695MPa, the total elongation under maximum force is 13.8%, the microstructure of the steel bar is ferrite + pearlite, and the grain size of the steel bar is grade 10. Figure 3 As shown in the 72-hour immersion accelerated corrosion test, the average corrosion rate is 3.2635 g / (m 2 ·h), the relative corrosion rate is 53.5%. Example 3
[0024] The production method and process conditions of this embodiment are exactly the same as those of Example 1. The chemical composition of the φ14mm 500MPa grade atmospheric corrosion resistant steel bar obtained is the same as that of Comparative Example 1, but the yield strength of the φ14mm steel bar is 520MPa, the tensile strength is 680MPa, and the total elongation under maximum force is 14.5%. Figure 2 As shown in the figure, the microstructure of the steel bar is ferrite and pearlite; the grain size of the steel bar is level 9, such as Figure 4 As shown in the 72-hour immersion accelerated corrosion test, the average corrosion rate is 3.995 g / (m 2 ·h), the relative corrosion rate is 65.5%. Example 4
[0025] The production method and process conditions of this embodiment are exactly the same as those of Example 2. The chemical composition of the φ14mm500MPa grade atmospheric corrosion resistant steel bar obtained is the same as that of Comparative Example 2, but the yield strength of the φ14mm steel bar is 540MPa, the tensile strength is 685MPa, the total elongation under maximum force is 13.2%, and the microstructure of the steel bar is ferrite and pearlite; the grain size of the steel bar is 10, such as Figure 4 As shown in the 72-hour immersion accelerated corrosion test, the average corrosion rate is 3.843 g / (m 2 ·h), the relative corrosion rate is 63%.
[0026] The 500MPa atmospheric corrosion resistant steel bar obtained by the production method increases the yield strength and tensile strength of the steel bar, improves the total elongation under maximum force and atmospheric corrosion resistance, and -2 mol / L NaHSO 3 In the accelerated corrosion test of 72 hours of immersion in the solution, the average corrosion rate was 3.2635-3.843g / (m 2 h), the relative corrosion rate is less than 70%.
Claims
1. A 500MPa grade atmospheric corrosion resistant steel bar, It is characterized in that The chemical composition, by mass percentage, includes: C: 0.18-0.21%, Si: 0.5-0.6%, Mn: 1.3-1.4%, Cu: 0.25-0.45%, P: 0.05-0.07%, S: 0.008-0.01%, V: 0.05-0.08%, Ti≤0.1%, Al≤0.1%, the balance is Fe and inevitable impurities. The microstructure of the steel bar is ferrite and pearlite, the grain size of the steel bar is grade 9-10, the yield strength of the steel bar is 515-550MPa, the tensile strength is 670-710MPa, and the total elongation under maximum force is 12-14.5%.
2. The method for producing the 500MPa grade atmospheric corrosion resistant steel bar according to claim 1, It is characterized in that The steps include: S1: Hot metal KR desulfurization: The hot metal conditions entering the furnace are controlled as follows: Si: 0.30-0.50%, P: ≤0.20%, S: ≤0.30%, temperature ≥1250℃. After the hot metal from the blast furnace arrives at the steelmaking workshop, CaO powder is sprayed into the hot metal ladle to promote the S in the hot metal to react with CaO to generate CaS, and then the CaS slag is removed by the slag removal equipment; S2: Primary refining in the converter: High-quality scrap steel is used to reduce the mixing of impurities. The copper plate is added into the furnace with the scrap steel at the lower limit. During the converter blowing process, the lance position is controlled by high-pull and supplementary blowing to control the process splashing. Slag materials are added during the converter blowing process, and the addition amount of slag materials per batch ≤ 500 Kg. The slag materials must be added within 3 minutes before the end point to achieve early slag melting in the initial stage and thorough slag melting in the process. The basicity of the final slag is controlled at R = 2.8 - 3.2, and the lance lowering time at the end point > 30 s. Bottom blowing nitrogen stirring is used in the early stage of the converter blowing process, and pure argon stirring is switched in the middle and later stages. End point control: 0.04% < C < 0.05%. Bottom blowing strong stirring is carried out at the end of blowing, and the flow rate is controlled at 200 M 3 The above ensures that the molten steel at the end point is not over-oxidized under the condition of low carbon; the tapping temperature of the converter is controlled between 1610°C and 1630°C, and the end point temperature can be increased by 10 - 30°C according to the ladle condition and abnormal situation; a ladle with good permeability and clean turnover of the porous plug is used. Bottom blowing nitrogen or argon is turned on 1 - 2 minutes before tapping. During the tapping process, large-air-volume stirring is carried out to ensure full melting of the alloy and ensure tapping with a hot ladle, and the ladle baking temperature > 900°C; slag blocking tapping is carried out to杜绝大量下渣,包内渣层厚度<50mm;脱氧合金化:放钢四分之一时,依次加入硅锰、复合脱氧剂、磷铁、钒氮合金,钢水出至四分之三时加完;出钢渣洗:出钢过程随钢流加入渣洗料,加入量为1~3 kg / t钢,加入时机为放钢四分之一时,随合金一起加入;出钢过程全程底吹氩搅拌,搅拌过程控制搅拌强度,钢包表面钢水裸露直径达到500mm,同时保证满足氩前温度要求;钢包到氩站中吹3分钟取样,调整成分后吹氩5分钟; S3: LF refining: When the ladle arrives at the refining site, the temperature is measured immediately and argon is passed. The argon pressure and flow rate are suitable for slightly turning the slag surface without exposing the molten steel. Lime + composite refining slag is used for slag making. During the refining process, the refining submerged arc operation is ensured to control the refining slag, quickly turn the slag into white slag, and perform soft argon blowing; S4: Billet continuous casting: control the superheat to 15-35℃; use magnesium dry material for the working layer of the tundish, and the baking temperature is ≥1000℃; use a long nozzle from the large ladle to the tundish and a sealing cover for the tundish to reduce temperature drop and secondary oxidation; use an aluminum-carbon immersion nozzle from the tundish to the crystallizer to ensure verticality and centering, and the insertion depth of the immersion nozzle is 90±10 mm; use a special protective slag for acid-resistant steel for the crystallizer protective slag, which must be dry and black-faced, and electromagnetic stirring is used during the production process; continuous casting cooling, the temperature before straightening is ≥900℃; ensure that the nozzle is not blocked, the water spray is uniform, and the position is centered to ensure the quality of the steel billet, and the surface is inspected and cleaned; S5: Heating: The temperature of the preheating section is ≤ 980°C. The heating temperature of the heating section and the soaking section is increased in the heating furnace. The furnace time is ≥ 120 min to ensure that the alloy elements V and Cu are fully and evenly dissolved in the austenite matrix. S6: Rolling: In the rolling process, micro-pile or micro-drawing rolling is adopted for rough rolling and intermediate rolling, and loop tension-free rolling is adopted for finishing rolling to avoid drawing steel rolling. Air cooling process is adopted after rolling to improve the strength of steel without sacrificing toughness, promote grain refinement, increase the yield strength and tensile strength of the material, improve the uniformity of the organization, and help to obtain a more uniform microstructure.
3. The method for producing a 500MPa grade atmospheric corrosion resistant steel bar according to claim 2, It is characterized in that The slag material in step S2 includes lime, dolomite and temperature regulating material, according to which lime accounts for 2 / 3 of the first batch, 1 / 3 of the later batch, all of dolomite, 3 / 4 of the temperature regulating material is added, and the rest is adjusted during "re-drying".
4. The method for producing a 500MPa grade atmospheric corrosion resistant steel bar according to claim 3, It is characterized in that The soft argon blowing time in step S3 must not be less than 8 minutes.
5. The method for producing 500MPa grade atmospheric corrosion resistant steel bars according to claim 4, It is characterized in that In step S4, the middle bag is a plugger bag or a sizing quick-change bag.
6. The method for producing 500MPa grade atmospheric corrosion resistant steel bars according to claim 5, It is characterized in that In step S4, the continuous casting cooling adopts a slow cooling mode.
7. The method for producing 500MPa grade atmospheric corrosion resistant steel bars according to claim 6, It is characterized in that In step S5, the temperature of the heating section is controlled at 1150°C to 1200°C.
8. The method for producing 500MPa grade atmospheric corrosion resistant steel bars according to claim 7, It is characterized in that In step S6, the starting rolling temperature of rough rolling is 1120°C to 1140°C, the starting rolling temperature of finishing rolling is 990°C to 1030°C, the final rolling temperature of finishing rolling is 1000°C to 1040°C, and the temperature of the upper cooling bed for air cooling is 990°C to 1000°C.
9. The method for producing 500MPa grade atmospheric corrosion resistant steel bars according to claim 8, It is characterized in that In step S6, pre-watering treatment is performed during the rolling process, and no watering is performed after rolling. The cooling rate of air cooling after rolling is controlled at 1-2°C / s.
Citation Information
Patent Citations
Vanadium and titanium compound microalloyed steel bar and production method thereof
CN102703813A
500MPa level corrosion resisting steel bar and production method
CN106756518A
High-strength atmospheric-corrosion-resistant steel bar and preparation method thereof
CN108193124A
Short flow 500 MPa level weather-resistant anti-seismic reinforcing steel bar and preparation method thereof
CN112458381A