Fuel cell metal bipolar plate coating resistant to high potential corrosion and long in service life and preparation method

By using closed non-equilibrium magnetic field coating furnace and magnetron sputtering technology on the metal bipolar plate of fuel cell, combined with graphite arc deposition technology, C coating with high sp3 bond ratio is prepared, which solves the poor corrosion resistance at high potential Problem, better corrosion resistance and stack output performance are achieved.

CN118910544APending Publication Date: 2024-11-08SUZHOU DONGFENG FINEBLANKING ENG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411012672.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing fuel cell metal bipolar plates have poor corrosion resistance at high potentials, resulting in increased contact resistance and reduced stack output power, and shortened life.

Method used

The coating furnace with closed non-equilibrium magnetic field and magnetron sputtering technology are used, combined with graphite arc deposition technology, and the C coating is prepared. The sp3 bond ratio and structural fineness of the C coating are improved through metal nitride transition coating, thereby enhancing the high Corrosion resistance at potential.

Benefits of technology

On the basis of ensuring the low-potential contact resistance performance, the corrosion resistance at high potential is significantly improved, the contact resistance change rate is reduced, and the life of the bipolar plate is extended.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910544A_ABST
    Figure CN118910544A_ABST
Patent Text Reader

Abstract

The invention discloses a high potential corrosion resistant long-life fuel cell metal bipolar plate coating and a preparation method thereof, the preparation method comprises the following steps: providing a coating furnace and a substrate, the coating furnace is provided with an anode layer ion source, a metal sputtering target and a graphite arc target; the coating furnace has a closed unbalanced magnetic field, and the graphite arc target has a magnetic filtering function; performing ultrasonic cleaning on the substrate; loading the substrate into a coating furnace, and adjusting the distance between the substrate and the target material; performing ion cleaning on the substrate by using an anode layer ion source; nitrogen is introduced into the coating furnace, the metal sputtering target and the substrate bias voltage are started, and a metal nitride coating is prepared; and starting the graphite arc target to prepare the C coating. The C coating prepared by the preparation method disclosed by the invention has good corrosion resistance under high potential on the premise of ensuring contact resistance and low-potential corrosion resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of surface modified coatings for fuel cell metal bipolar plates, and in particular to a high potential corrosion resistant and long-life fuel cell metal bipolar plate coating and a preparation method thereof. Background Art

[0002] Bipolar plates are the core components of proton exchange membrane fuel cells. They play important roles in the fuel cell stack, such as structural support, separation of hydrogen and oxygen, heat conduction, electrical conduction, and provision of hydrogen and oxygen channels. Metal bipolar plates are widely used due to their low cost and short processing cycle. The base material of metal bipolar plates is usually Ti or 316L stainless steel, which is prone to corrosion in the fuel cell environment, causing bipolar plate penetration and battery damage and scrapping.

[0003] The usual method is to use vacuum coating technology to prepare a corrosion-resistant and conductive coating on the surface of the metal bipolar plate. Common coating materials include Ti / Nb / Cr / Ta / W and its nitrides, Au, C, etc. Among them, the C coating has become one of the current mainstream coatings due to its superior performance and low cost.

[0004] Common preparation methods for C coatings include magnetron sputtering, multi-arc ion plating, etc. 2 Key and sp 3 The bonds exist in a certain proportion, and different proportions can make the coating present different properties. At present, the contact resistance performance of C coating on the market is good, and most of them can reach ≤5mΩ·cm under 1.0Mpa. 2 , the purpose is to ensure the output power of the battery stack; at the same time, the corrosion resistance at low potential can meet most working conditions, for example, the corrosion current density at 0.8V (SHE) potential in a PH=3 environment is ≤1μA / cm 2 However, when facing the extremely high potential conditions of the battery stack during start-up, shutdown, activation, etc., the corrosion resistance of most C coatings is poor. For example, at 1.6V (SHE), the corrosion current density is usually 100μA / cm 2 The contact resistance after high potential corrosion also increased significantly. For example, the contact resistance after 1.6V / 10H corrosion increased to 20mΩ·cm 2 If the contact resistance change rate is above 300%, it will greatly reduce the subsequent output power and life of the battery stack. Summary of the invention

[0005] In order to solve the above technical problems, the purpose of the present invention is to provide a high-potential corrosion-resistant and long-life fuel cell metal bipolar plate coating and a preparation method thereof. The C coating prepared by the preparation method of the present invention has good corrosion resistance at high potential while ensuring contact resistance and low-potential corrosion resistance.

[0006] In order to achieve the above technical objectives and the above technical effects, the present invention is implemented through the following technical solutions:

[0007] In one aspect, the present invention provides a method for preparing a high-potential corrosion-resistant and long-life fuel cell metal bipolar plate coating, comprising the following steps:

[0008] (1) providing a coating furnace and a substrate, wherein the coating furnace is provided with an anode layer ion source, a metal sputtering target, and a graphite arc target; the coating furnace has a closed non-equilibrium magnetic field, and the graphite arc target has a magnetic filtering function;

[0009] (2) ultrasonically cleaning the substrate;

[0010] (3) Loading the substrate into the coating furnace and adjusting the distance between the substrate and the target;

[0011] (4) using an anode layer ion source to perform ion cleaning on the substrate;

[0012] (5) introducing nitrogen into the coating furnace, turning on the metal sputtering target and substrate bias, and preparing the metal nitride coating;

[0013] (6) Turn on the graphite arc target to prepare the C coating.

[0014] Furthermore, in step (2), after ultrasonic cleaning, the surface dyne value of the substrate is ≥52.

[0015] Furthermore, in step (3), the distance between the target and the substrate is 70 mm to 160 mm.

[0016] Furthermore, in step (4), the ion cleaning process is as follows: the coating furnace is vacuumed to 1×10 -1 When the temperature is below pa, the furnace chamber is heated to 80℃~200℃, Ar gas is introduced, and the anode layer ion source and substrate bias are turned on. + The substrate was ion cleaned for 30 min.

[0017] Furthermore, in step (5), after the ion cleaning is completed, the furnace chamber temperature is maintained at 80°C to 200°C, Ar and N2 gases are introduced, the metal sputtering target and substrate bias are turned on, and the metal nitride coating is prepared.

[0018] Furthermore, in step (5), the gas flow ratio of Ar and N2 is 15:1 to 15:15, the gas pressure is 0.5 Pa to 1 Pa, the sputtering power is 1 KW to 5 KW, and the bias voltage is -50 V to -300 V.

[0019] Furthermore, in step (6), after the preparation of the metal nitride coating is completed, the furnace chamber heating is turned off, and after the temperature is ≤80°C, Ar gas is introduced and the graphite arc target is turned on to prepare the C coating; the gas pressure in this step is 0.2Pa~1Pa, the target current is 50A~100A, the substrate bias is -50V~-200V, and the substrate bias current is 5A~20A.

[0020] Another aspect of the present invention provides a high potential corrosion resistant and long life fuel cell metal bipolar plate coating, comprising a transition coating disposed on a substrate and a C coating disposed on the transition coating; the transition coating is a metal nitride coating, and the C coating is composed of sp 2 and sp 3 The amorphous structure composed of valence C, in which sp 3 The key ratio is 45%-75%.

[0021] Furthermore, the material of the transition coating is a metal nitride formed by nitrogen and any one of metals Ti, Nb, Cr, Ta, and W.

[0022] Furthermore, the thickness of the transition coating is 50nm-600nm, and the nitrogen atom:metal atom=0.1-0.3; the thickness of the C coating is 50nm-400nm.

[0023] The beneficial effects of the present invention are:

[0024] The furnace body of the coating furnace in the preparation method of the present invention has a closed non-equilibrium magnetic field, which, combined with specific parameters in the magnetron sputtering and arc deposition processes, can greatly improve the ionization rate, make the arc spots more refined, the particles smaller and fewer, and the prepared coating more delicate.

[0025] The present invention adopts a graphite arc target, which has a magnetic filtering function. With the cooperation of a specific target current, substrate bias voltage, and substrate bias current, large particles in the coating can be reduced and the coating performance can be improved.

[0026] The C coating prepared by the preparation method of the present invention has good corrosion resistance at high potential while ensuring contact resistance and low potential corrosion resistance.

[0027] The properties of the bipolar plate coating of the present invention are as follows:

[0028] 1. Contact resistance at 1.0MPa <3mΩ·cm 2 ;

[0029] 2. Potential dynamic corrosion current density 0.6V<0.5μA / cm 2 ;

[0030] 3. 1.4V / 10H corrosion current density <15μA / cm 2;

[0031] 4. After 1.4V / 10H corrosion, the contact resistance is less than 4mΩ·cm 2 ;

[0032] 5. After 1.4V / 10H corrosion, the contact resistance change rate is less than 50%. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 It is a schematic diagram of the structure of the fuel cell metal bipolar plate coating of the present invention.

[0034] In the figure, 1: substrate; 2: transition coating; 3: C coating. DETAILED DESCRIPTION

[0035] The preferred embodiments of the present invention are described in detail below in conjunction with the accompanying drawings so that the advantages and features of the present invention can be more easily understood by those skilled in the art, thereby making a clearer and more definite definition of the protection scope of the present invention.

[0036] A method for preparing a high-potential corrosion-resistant and long-life fuel cell metal bipolar plate coating comprises the following steps:

[0037] (1) providing a coating furnace and a substrate, wherein the coating furnace is provided with an anode layer ion source, a metal sputtering target, and a graphite arc target; the purity of the target material is ≥ 99.7%; the coating furnace has a closed non-equilibrium magnetic field, and the graphite arc target has a magnetic filtering function; the material of the substrate is Ti or 316L stainless steel;

[0038] (2) ultrasonically clean the substrate to make the surface dyne value ≥52;

[0039] (3) Loading the ultrasonically cleaned substrate into the coating furnace, and adjusting the distance between the substrate and the target to 70 mm to 160 mm;

[0040] (4) Using the anode layer ion source to perform ion cleaning on the substrate; the specific process of ion cleaning is as follows: the coating furnace is vacuumed to 1×10 -1 When the temperature is below pa, the furnace chamber is heated to 80℃~200℃, Ar gas is introduced, and the ion source and substrate bias are turned on. + The substrate was ion cleaned for 30 min;

[0041] (5) After the ion cleaning is completed, the furnace chamber temperature is maintained at 80°C to 200°C, Ar and N2 gases are introduced, the metal sputtering target and the substrate bias are turned on, and a metal nitride coating is prepared; wherein the gas flow ratio Ar:N2 is 15:1 to 15:15; the process gas pressure is 0.5Pa to 1Pa; the sputtering power is 1KW to 5KW; the bias voltage is -50V to -300V; in the prepared metal nitride coating, nitrogen atoms: metal atoms = 0.1 to 0.3; the thickness of the metal nitride coating is 50nm to 600nm;

[0042] (6) After the preparation of the metal nitride coating, the furnace chamber heating is turned off. When the temperature is ≤80°C, Ar gas is introduced, and the graphite arc target is turned on to start preparing the C coating; the process gas pressure is 0.2Pa~1Pa; the target current is 50A~100A; the substrate bias voltage is -50V~-200V; the substrate bias current is 5A~20A; the sp in the C coating is 3 The bond ratio is 45%-75%; the thickness is 50nm~400nm.

[0043] like Figure 1 As shown, the high potential corrosion resistant and long life fuel cell metal bipolar plate coating prepared by the preparation method of the present invention comprises a transition coating 2 arranged on a substrate 1 and a C coating 3 arranged on the transition coating 2; the transition coating 2 is a metal nitride coating, and the C coating 3 is a sp 2 and sp 3 Amorphous structure composed of valence C, sp 3 The bond ratio is 45%-75%. The substrate material is Ti or 316L stainless steel; the transition coating material is a metal nitride composed of nitrogen and any one of metals Ti, Nb, Cr, Ta, and W. The thickness of the transition coating (metal nitride coating) 2 is 50nm-600nm, and the nitrogen atom: metal atom = 0.1-0.3; the thickness of the C coating 3 is 50nm-400nm.

[0044] The coating obtained by the preparation method of the present invention is tested for performance

[0045] Refer to "GB / T 20042.6-2024 Proton Exchange Membrane Fuel Cell Part 6: Bipolar Plate Characteristics Test Method"; the test conditions are:

[0046] 1. Contact resistance: detection area 4cm 2 , loading pressure 1.0MPa, carbon paper is TGP-H-060;

[0047] 2. Potential dynamic corrosion current density @0.6V: detection area 4cm 2, the solution is PH=3 sulfuric acid + 5ppm hydrofluoric acid, the solution temperature is 80℃, the air is introduced at 20ml / min, and the reference electrode is Ag / AgCl;

[0048] 3. 1.4V / 10H corrosion current density: detection area 4cm 2 , the solution is PH=3 sulfuric acid + 5ppm hydrofluoric acid, the solution temperature is 80℃, the air is introduced at 20ml / min, and the reference electrode is Ag / AgCl;

[0049] 4. Contact resistance change rate: The contact resistance of the sample before 1.4V / 10H corrosion is R1, and the contact resistance after corrosion is R2, and the change rate = (R2-R1) / R1×100%;

[0050] The test results are:

[0051] (1) Contact resistance at 1.0MPa <3mΩ·cm 2 ;

[0052] (2) Potentiodynamic corrosion current density 0.6V<0.5μA / cm 2 ;

[0053] (3) 1.4V / 10H corrosion current density <15μA / cm 2 ;

[0054] (4) After 1.4V / 10H corrosion, contact resistance <4mΩ·cm 2 ;

[0055] (5) After 1.4V / 10H corrosion, the contact resistance change rate is less than 50%;

[0056] Example 1

[0057] The 316L substrate was cleaned with ultrasonic waves, and the surface dyne value after cleaning was 52. The coating furnace was equipped with an ion source, a Ti sputtering target, and a graphite arc target, and the purity of the target material was 99.99%. The furnace body had a closed non-equilibrium magnetic field, and the graphite arc target had a magnetic filtering function. The ultrasonically cleaned substrate was loaded into the coating furnace, and the distance between the target and the substrate was adjusted to 80 mm. The vacuum of the coating furnace was drawn to 5×10 -2 At 1 pa, the furnace chamber was heated to 100 °C, Ar gas was introduced, and the ion source and substrate bias were turned on. The ion source current was 1A, the substrate bias was -500V, and Ar was used to generate the +The substrate was ion cleaned for 30 minutes. After ion cleaning, the furnace temperature was maintained at 100°C, Ar and N2 gases were introduced, the metal sputtering Ti target and substrate bias were turned on, and the metal nitride coating was prepared; the thickness of the metal nitride coating was 150nm. After the preparation of the metal nitride coating, the furnace heating was turned off, and when the temperature was ≤80°C, Ar gas was introduced, and the graphite arc target was turned on to start preparing the C coating; the process gas pressure was 0.25pa; the target current was 80A; the coil current of the filter magnetic field was 0.5A; the substrate bias was -100V; the substrate bias current was 12A; the sp3 bond ratio in the prepared C coating was 68%, and the coating thickness was 200nm.

[0058] After the coating is prepared, the contact resistance and corrosion current of the substrate are tested in accordance with GB / T 20042.6-2024 Proton Exchange Membrane Fuel Cell Part 6: Bipolar Plate Characteristics Test Method. The test conditions are as follows:

[0059] 1. Contact resistance: detection area 4cm 2 , loading pressure 1.0MPa, carbon paper is TGP-H-060

[0060] 2. Potential dynamic corrosion current density @0.6V: detection area 4cm 2 , the solution is PH=3 sulfuric acid + 5ppm hydrofluoric acid, the solution temperature is 80℃, the air is introduced at 20ml / min, and the reference electrode is Ag / AgCl;

[0061] 3. 1.4V / 10H corrosion current density: detection area 4cm2, solution PH=3 sulfuric acid + 5ppm hydrofluoric acid, solution temperature 80℃, air flow 20ml / min, reference electrode is Ag / AgCl;

[0062] The test results are:

[0063] 1. The contact resistance is 2.2mΩ·cm at 1.0MPa 2 ;

[0064] 2. Potential dynamic corrosion current density @0.6V is 0.43μA / cm 2 ;

[0065] 3. 1.4V / 10H corrosion current density is 12.2μA / cm 2 ;

[0066] 4. After 1.4V / 10H corrosion, the contact resistance is 3.2mΩ·cm 2 ;

[0067] 5. After 1.4V / 10H corrosion, the contact resistance change rate is 45%.

[0068] Example 2

[0069] The difference between this embodiment and the first embodiment is that the metal sputtering target is a Nb target material with a purity of 99.99%.

[0070] The test results of the prepared coating are:

[0071] 1. The contact resistance is 1.8mΩ·cm at 1.0MPa 2 ;

[0072] 2. Potential dynamic corrosion current density @0.6V is 0.48μA / cm 2 ;

[0073] 3. 1.4V / 10H corrosion current density is 13.5μA / cm 2 ;

[0074] 4. After 1.4V / 10H corrosion, the contact resistance is 2.5mΩ·cm 2 ;

[0075] 5. After 1.4V / 10H corrosion, the contact resistance change rate is 39%.

[0076] Example 3

[0077] The difference between this embodiment and embodiment 1 is that when preparing the C coating, the graphite arc target current is 60A, the magnetic filter coil current is 1A, and the substrate bias voltage is -60V.

[0078] The test results of the prepared coating are:

[0079] 1. The contact resistance is 2.5mΩ·cm at 1.0MPa 2 ;

[0080] 2. Potential dynamic corrosion current density @0.6V is 0.35μA / cm 2 ;

[0081] 3. 1.4V / 10H corrosion current density is 14.6μA / cm 2 ;

[0082] 4. After 1.4V / 10H corrosion, the contact resistance is 3.3mΩ·cm 2 ;

[0083] 5. After 1.4V / 10H corrosion, the contact resistance change rate is 28%.

[0084] Example 4

[0085] The difference between this embodiment and embodiment 1 is that the substrate material is Ti, and the preparation process is the same as that of embodiment 1.

[0086] The test results of the prepared coating are:

[0087] 1. The contact resistance is 2.3mΩ·cm at 1.0MPa 2 ;

[0088] 2. Potential dynamic corrosion current density @0.6V is 0.55μA / cm 2 ;

[0089] 3. 1.4V / 10H corrosion current density is 10.5μA / cm 2 ;

[0090] 4. After 1.4V / 10H corrosion, the contact resistance is 2.8mΩ·cm 2 ;

[0091] 5. After 1.4V / 10H corrosion, the contact resistance change rate is 22%.

[0092] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.

[0093] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A method for preparing a high potential corrosion resistant and long life fuel cell metal bipolar plate coating, characterized in that: The steps include: (1) providing a coating furnace and a substrate, wherein the coating furnace is provided with an anode layer ion source, a metal sputtering target, and a graphite arc target; the coating furnace has a closed non-equilibrium magnetic field, and the graphite arc target has a magnetic filtering function; (2) ultrasonically cleaning the substrate; (3) Loading the substrate into the coating furnace and adjusting the distance between the substrate and the target; (4) using an anode layer ion source to perform ion cleaning on the substrate; (5) introducing nitrogen into the coating furnace, turning on the metal sputtering target and substrate bias, and preparing the metal nitride coating; (6) Turn on the graphite arc target to prepare the C coating.

2. The method for preparing a high potential corrosion resistant and long life fuel cell metal bipolar plate coating according to claim 1, characterized in that: In step (2), after ultrasonic cleaning, the surface dyne value of the substrate is ≥52.

3. The method for preparing a high potential corrosion resistant and long life fuel cell metal bipolar plate coating according to claim 1, characterized in that: In step (3), the distance between the target and the substrate is 70 mm to 160 mm.

4. The method for preparing a high potential corrosion resistant and long life fuel cell metal bipolar plate coating according to claim 1, characterized in that: In step (4), the ion cleaning process is as follows: the coating furnace is vacuumed to 1×10 -1 When the temperature is below pa, the furnace chamber is heated to 80℃~200℃, Ar gas is introduced, and the anode layer ion source and substrate bias are turned on. + The substrate was ion cleaned for 30 min.

5. The method for preparing a high potential corrosion resistant and long life fuel cell metal bipolar plate coating according to claim 1, characterized in that: In step (5), after the ion cleaning is completed, the furnace chamber temperature is maintained at 80°C to 200°C, Ar and N2 gases are introduced, the metal sputtering target and substrate bias are turned on, and the metal nitride coating is prepared.

6. The method for preparing a high potential corrosion resistant and long life fuel cell metal bipolar plate coating according to claim 5, characterized in that: In step (5), the gas flow ratio of Ar and N2 is 15:1 to 15:15, the gas pressure is 0.5 Pa to 1 Pa, the sputtering power is 1 KW to 5 KW, and the bias voltage is -50 V to -300 V.

7. The method for preparing a high potential corrosion resistant and long life fuel cell metal bipolar plate coating according to claim 1, characterized in that: In step (6), after the preparation of the metal nitride coating is completed, the furnace chamber heating is turned off, and when the temperature is ≤80°C, Ar gas is introduced and the graphite arc target is turned on to prepare the C coating; the gas pressure in this step is 0.2Pa~1Pa, the target current is 50A~100A, the substrate bias is -50V~-200V, and the substrate bias current is 5A~20A.

8. A high potential corrosion resistant and long life fuel cell metal bipolar plate coating, characterized in that: It includes a transition coating disposed on a substrate and a C coating disposed on the transition coating; the transition coating is a metal nitride coating, and the C coating is composed of sp 2 and sp 3 The amorphous structure composed of valence C, in which sp 3 The key ratio is 45%-75%.

9. The high potential corrosion resistant and long life fuel cell metal bipolar plate coating according to claim 8, characterized in that: The material of the transition coating is a metal nitride formed by nitrogen and any one of metals Ti, Nb, Cr, Ta and W.

10. The high potential corrosion resistant and long life fuel cell metal bipolar plate coating according to claim 8, characterized in that: The thickness of the transition coating is 50nm-600nm, and the ratio of nitrogen atoms to metal atoms is 0.1-0.3; the thickness of the C coating is 50nm-400nm.