Recycling method of titanium-aluminum alloy target material
Through vacuum suspension smelting and thermal isostatic pressing, the impurities, difficulty and cost problems in the preparation of titanium-aluminum alloy targets are solved, and the high purity and composition uniformity of the titanium-aluminum alloy targets are achieved efficiently recycling, which is suitable for large-scale Promote application.
Patent Information
- Application Number
- CN202411005537.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing titanium-aluminum alloy target preparation methods have problems such as high impurity content, high powder metallurgy requirements, high preparation difficulty, high cost, smelting defects, and ingredient segregation. The remaining materials cannot be efficiently recycled and processed after the target is used, resulting in Higher cost.
Using vacuum suspension smelting combined with thermal isostatic pressure, the residual titanium-aluminum alloy targets are pretreated, cleaned, mixed, vacuum suspension smelting and thermal isostatic pressure to achieve efficient recovery of titanium-aluminum alloy targets and improve the recovery rate of metal elements. , eliminate internal defects and uneven composition problems.
It achieves high purity, composition uniformity and tissue uniformity of titanium-aluminum alloy targets, shortens the processing cycle, reduces the recycling cost, and is suitable for large-scale applications.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of target material recycling and processing, and specifically relates to a method for recycling a titanium-aluminum alloy target material. Background Art
[0002] Titanium aluminum alloy target is an alloy sputtering target for vacuum coating. Titanium aluminum alloy targets with different properties can be obtained by adjusting the ratio of titanium to aluminum. Titanium aluminum alloy has good wear resistance and good application prospects in the mechanical processing industry, but it is hard and brittle, has poor process performance, complex preparation process, and long production cycle. It is a typical difficult-to-process and difficult-to-prepare material.
[0003] At present, the preparation methods of titanium aluminum alloy targets mainly include powder metallurgy and smelting. CN111575659A discloses a preparation method of titanium aluminum alloy target, which includes the following steps: providing titanium aluminum alloy target raw material powder: mixing the titanium aluminum alloy target raw material powder evenly according to proportion to obtain blank powder; crushing the blank powder in a protective gas atmosphere to obtain powder: mixing the powder and the bonding coating agent, granulating, pressing and forming, and obtaining a preform; debonding the preform in a reducing atmosphere, hot pressing and sintering, and obtaining a titanium aluminum alloy target. However, this method still has difficulty in solving the problem of high impurity content, and the powder metallurgy method has high requirements for powder, and the preparation is difficult.
[0004] CN104651662A discloses a vacuum induction melting method for titanium-aluminum alloy target material. The method uses a CaO crucible for vacuum induction melting to prepare titanium-aluminum alloy, and sequentially includes a batching step, a baking step, a furnace loading step, an alloy melting step, and a casting step. However, the use of vacuum induction melting to prepare titanium-aluminum alloy target material still needs to further solve the problems of melting defects, component segregation, impurities, and molding from ingot to target material.
[0005] The use of the above-mentioned traditional powder metallurgy and smelting methods to prepare titanium aluminum alloy targets not only has quality and complex process problems, but also faces the problem of high cost. After the target is used, a large amount of material is often left unsputtered. If these remaining materials can be recycled in an efficient and low-cost method, the cost of target preparation will be greatly reduced.
[0006] Therefore, if a method for recycling titanium aluminum alloy targets is provided to improve the recovery rate of metal elements in the targets, avoid the introduction of impurities, obtain targets with internal defects, shorten the processing cycle, and reduce the recycling cost, it has become an urgent problem that technical personnel in this field need to solve. Summary of the invention
[0007] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a method for recycling titanium-aluminum alloy targets. The method comprises vacuum suspension melting of titanium-aluminum alloy residual targets and hot isostatic pressing for post-processing of the target blanks to obtain titanium-aluminum alloy targets with high purity and uniform composition and structure; and the method has a short production cycle and high efficiency, which is conducive to large-scale promotion and application.
[0008] To achieve this object, the present invention adopts the following technical solutions:
[0009] The present invention provides a method for recycling a titanium-aluminum alloy target material, and the recycling method comprises the following steps:
[0010] (1) pretreating a titanium-aluminum alloy residual target to obtain a titanium-aluminum alloy target block;
[0011] (2) sequentially pickling, water washing, organic solvent cleaning and vacuum drying the titanium aluminum alloy target block obtained in step (1) to obtain a decontaminated target block;
[0012] (3) The impurity-removed target block obtained in step (2) is sequentially subjected to mixing, vacuum suspension melting, casting and hot isostatic pressing to obtain the titanium-aluminum alloy target material.
[0013] The recycling method provided by the present invention realizes efficient recycling of titanium-aluminum alloy residual targets through pretreatment, cleaning process, vacuum suspension melting and hot isostatic pressing performed in sequence; the pretreatment processes the complete titanium-aluminum alloy residual targets into titanium-aluminum alloy target blocks suitable for subsequent processes; the cleaning process avoids the introduction of impurities and improves the purity of the titanium-aluminum alloy obtained by smelting; the vacuum suspension melting fully recovers the target metal elements in the titanium-aluminum alloy residual targets and significantly improves the recovery rate of the metal elements in the target material; the hot isostatic pressing can effectively eliminate the internal defects of the target material and the problems of uneven organizational composition; the recycling method provided by the present invention has a short processing cycle and low recycling cost, which is conducive to large-scale promotion and application.
[0014] As a preferred technical solution of the present invention, the proportion of aluminum element in the titanium-aluminum alloy residual target in step (1) is 35-37wt%, for example, it can be 35wt%, 35.4wt%, 35.8wt%, 36.2wt%, 36.6wt% or 37wt%, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0015] As a preferred technical solution of the present invention, the preprocessing includes turning processing and splitting processing performed in sequence.
[0016] Preferably, the turning process is to remove the backing plate and the sputtering layer on the surface of the titanium-aluminum alloy residual target.
[0017] Preferably, during the separation of the titanium-aluminum alloy residual target and the backing plate, the processing position of the turning process is 1 to 3 mm lower than the welding line of the titanium-aluminum alloy residual target, for example, it can be 1 mm, 1.4 mm, 1.8 mm, 2.2 mm, 2.6 mm or 3 mm, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0018] In the present invention, the machining position of the turning process is 1 to 3 mm lower than the welding line of the residual target of the titanium-aluminum alloy, which is beneficial to reducing the introduction of impurities during the smelting process and improving the purity of the titanium-aluminum alloy.
[0019] Preferably, the segmentation process is to make the length, width and thickness of the titanium aluminum alloy target block all 20 to 40 mm, for example, 20 mm, 24 mm, 28 mm, 32 mm, 36 mm or 40 mm, but not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0020] As a preferred technical solution of the present invention, the acid solution used for pickling in step (2) is composed of nitric acid, hydrofluoric acid and water in a molar ratio of 1 to 2:1:4.5 to 5.5, for example, it can be 1:1:5, 2:1:4.5, 1.5:1:5.5 or 1:1:4.5, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0021] Preferably, the pickling time is 15 to 30 minutes, for example, 15 minutes, 18 minutes, 21 minutes, 24 minutes, 27 minutes or 30 minutes, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0022] Preferably, the organic solvent in the organic solvent cleaning in step (2) comprises any one of isopropanol, acetone or ethanol, or a combination of at least two of them. Typical but non-limiting combinations include: a combination of isopropanol and acetone, a combination of acetone and ethanol, a combination of isopropanol and ethanol, or a combination of isopropanol, acetone and ethanol.
[0023] Preferably, the time for washing with the organic solvent in step (2) is 10 to 15 minutes, for example, 10 minutes, 11 minutes, 12 minutes, 13 minutes, 14 minutes or 15 minutes, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0024] Preferably, the organic solvent cleaning in step (2) is carried out under ultrasonic conditions.
[0025] As a preferred technical solution of the present invention, the vacuum drying temperature in step (2) is 100-150°C, for example, it can be 100°C, 110°C, 120°C, 130°C, 140°C or 150°C, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0026] Preferably, the vacuum drying time in step (2) is 2 to 3 h, for example, 2 h, 2.1 h, 2.2 h, 2.3 h, 2.4 h, 2.5 h, 2.6 h, 2.7 h, 2.8 h, 2.9 h or 3 h, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0027] Preferably, the vacuum drying in step (2) further includes a cooling treatment.
[0028] As a preferred technical solution of the present invention, the mixed material in step (3) includes mixing high-purity aluminum particles and the impurity-removed target block obtained in step (2).
[0029] Preferably, the added amount of the high-purity aluminum particles is 0.7-0.8wt% of the mass of the de-doping target block, for example, it can be 0.7wt%, 0.72wt%, 0.74wt%, 0.76wt%, 0.78wt% or 0.8wt%, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0030] Preferably, the purity of the high-purity aluminum particles is ≥99.999%, for example, it can be 99.999%, 99.9992%, 99.9994%, 99.9996% or 99.9998%, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0031] In the present invention, high-purity aluminum particles are mixed before smelting to supplement the aluminum burnout during the smelting process. If the amount of aluminum added is too high, it will lead to excessive aluminum and generate alloy phases such as TiAl3 and TiAl2. If it is too low, it will lead to excessive Ti and produce Ti3Al alloy phase.
[0032] As a preferred technical solution of the present invention, the vacuum degree of the vacuum suspension smelting in step (3) is ≤0.05Pa, for example, it can be 0.05Pa, 0.04Pa, 0.03Pa, 0.02Pa or 0.01Pa, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0033] Preferably, the temperature of the vacuum suspension melting in step (3) is 1500-1550°C, for example, it can be 1500°C, 1510°C, 1520°C, 1530°C, 1540°C or 1550°C, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0034] In the present invention, the role of the vacuum suspension smelting is that the smelting process is carried out in a vacuum, and the electromagnetic force is used to support the molten metal. The molten metal is not contaminated by the crucible, and the purity of the titanium aluminum alloy is further improved. Too high a temperature will cause excessive metal burning, and too low a temperature will result in the material not being completely melted.
[0035] Preferably, the vacuum suspension melting time in step (3) is 15 to 30 minutes, for example, 15 minutes, 18 minutes, 21 minutes, 24 minutes, 27 minutes or 30 minutes, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0036] As a preferred technical solution of the present invention, the pressure of the hot isostatic pressing in step (3) is 150-180 MPa, for example, it can be 150 MPa, 155 MPa, 160 MPa, 165 MPa, 170 MPa, 175 MPa or 180 MPa, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0037] Preferably, the temperature of the hot isostatic pressing in step (3) is 1250-1300°C, for example, it can be 1250°C, 1260°C, 1270°C, 1280°C, 1290°C or 1300°C, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0038] The present invention adopts hot isostatic pressing process to eliminate the problems of internal defects and uneven tissue composition of the target material; if the temperature is too high, the material will undergo phase change, so that the final tissue does not meet the requirements; if the temperature is too high, the material will melt; if the temperature is too low, the elements cannot diffuse fully; in addition, if the temperature is too low, the material gamma phase change zone cannot be reached; if the pressure is too high, the equipment carrying capacity will be exceeded; if the pressure is too low, some defects cannot be completely closed, and the material defect rate is high.
[0039] Preferably, the hot isostatic pressing time in step (3) is 240 to 360 min, for example, 240 min, 270 min, 300 min, 330 min or 360 min, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0040] As a preferred technical solution of the present invention, the purity of the titanium aluminum alloy target is greater than 99.99%, for example, it can be 99.992%, 99.994%, 99.996% or 99.998%, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0041] Preferably, the titanium aluminum alloy target has a single γ phase.
[0042] As a preferred technical solution of the present invention, the method for recycling the titanium aluminum alloy target material of the present invention comprises the following steps:
[0043] (1) turning a titanium-aluminum alloy residual target in which the aluminum element accounts for 35 to 37 wt % to remove a back plate and a sputtering layer on the surface of the titanium-aluminum alloy residual target, and then cutting the target to obtain a titanium-aluminum alloy target block having a length, width and thickness of 20 to 40 mm;
[0044] (2) The titanium aluminum alloy target block obtained in step (1) is sequentially pickled with an acid solution composed of nitric acid, hydrofluoric acid and water in a molar ratio of 1 to 2:1:4.5 to 5.5 for 15 to 30 minutes, washed with water, and cleaned with an organic solvent in an ultrasonic wave for 10 to 15 minutes, vacuum dried at 100 to 150° C. for 2 to 3 hours, and then cooled to obtain a de-impurified target block;
[0045] (3) High-purity aluminum particles with an addition amount of 0.7-0.8 wt% of the mass of the impurity-removed target block and the impurity-removed target block obtained in step (2) are mixed, and then vacuum suspension melting is performed for 15-30 min at a vacuum degree of ≤0.05 Pa and 1500-1550° C. After casting, hot isostatic pressing is performed for 240-360 min at 150-180 MPa and 1250-1300° C. to obtain a titanium aluminum alloy target with a purity of >99.99% and a single γ phase.
[0046] The following are preferred technical solutions of the present invention, but are not intended to limit the technical solutions provided by the present invention. Through the following preferred technical solutions, the objectives and beneficial effects of the present invention can be better achieved and realized.
[0047] Compared with the prior art, the present invention has the following beneficial effects:
[0048] (1) The recycling method of the titanium aluminum alloy target provided by the present invention adopts vacuum suspension melting to remove impurities from the target block, and simultaneously introduces hot isostatic pressing to treat the titanium aluminum alloy, which is beneficial to eliminate internal defects and uneven organizational composition.
[0049] (2) The titanium-aluminum alloy target material recycling method provided by the present invention has a short production cycle and high efficiency. The obtained titanium-aluminum alloy target material has high purity, uniform composition and structure, and no internal defects, and can be reused as a sputtering material. DETAILED DESCRIPTION
[0050] For the convenience of understanding the present invention, the present invention lists the following embodiments. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0051] Example 1
[0052] This embodiment provides a method for recycling a titanium aluminum alloy target material, and the recycling method comprises the following steps:
[0053] (1) performing a turning process on a titanium-aluminum alloy residual target in which the aluminum element accounts for 36 wt % to remove the back plate and the sputtering layer on the surface of the titanium-aluminum alloy residual target, and then performing a cutting process to obtain a titanium-aluminum alloy target block with a length, width and thickness of 30 mm;
[0054] (2) The titanium aluminum alloy target block obtained in step (1) is sequentially pickled with an acid solution composed of nitric acid, hydrofluoric acid and water in a molar ratio of 1 to 2:1:5 for 22 minutes, washed with water, and cleaned with isopropanol in an ultrasonic wave for 12.5 minutes, vacuum dried at 125° C. for 2.5 hours, and then cooled to obtain a decontaminated target block;
[0055] (3) High-purity aluminum particles with an addition amount of 0.75 wt% of the mass of the impurity-removed target block and the impurity-removed target block obtained in step (2) are mixed, and then vacuum suspension melting is performed for 25 min at a vacuum degree of 0.04 Pa and 1525° C. After casting, hot isostatic pressing is performed for 310 min at 170 MPa and 1275° C. to obtain a titanium aluminum alloy target.
[0056] Example 2
[0057] This embodiment provides a method for recycling a titanium aluminum alloy target material, and the recycling method comprises the following steps:
[0058] (1) turning a titanium-aluminum alloy residual target in which the aluminum element accounts for 35 wt % to remove the back plate and the sputtering layer on the surface of the titanium-aluminum alloy residual target, and then cutting to obtain a titanium-aluminum alloy target block with a length, width and thickness of 20 mm;
[0059] (2) The titanium aluminum alloy target block obtained in step (1) was pickled with an acid solution composed of nitric acid, hydrofluoric acid and water in a molar ratio of 1:1:4.5 for 15 minutes, washed with water and cleaned with acetone in an ultrasonic wave for 10 minutes, vacuum dried at 100° C. for 3 hours, and then cooled to obtain a decontaminated target block;
[0060] (3) High-purity aluminum particles with an addition amount of 0.7 wt% of the mass of the impurity-removed target block and the impurity-removed target block obtained in step (2) are mixed, and then vacuum suspension melting is carried out at a vacuum degree of 0.05 Pa and 1500°C for 30 min. After casting, hot isostatic pressing is carried out at 150 MPa and 1250°C for 240 min to obtain a pure titanium aluminum alloy target.
[0061] Example 3
[0062] This embodiment provides a method for recycling a titanium aluminum alloy target material, and the recycling method comprises the following steps:
[0063] (1) turning a titanium-aluminum alloy residual target in which the aluminum element accounts for 37 wt % to remove the back plate and the sputtering layer on the surface of the titanium-aluminum alloy residual target, and then cutting to obtain a titanium-aluminum alloy target block with a length, width and thickness of 40 mm;
[0064] (2) The titanium aluminum alloy target block obtained in step (1) was pickled with an acid solution composed of nitric acid, hydrofluoric acid and water in a molar ratio of 2:1:5.5 for 30 minutes, washed with water, and cleaned with an organic solvent in an ultrasonic wave for 15 minutes, vacuum dried at 150° C. for 2 hours, and then cooled to obtain a de-impurified target block;
[0065] (3) High-purity aluminum particles with an addition amount of 0.8 wt% of the mass of the impurity-removed target block and the impurity-removed target block obtained in step (2) are mixed, and then vacuum suspension melting is performed for 15 min at a vacuum degree of 0.01 Pa and 1550°C. After casting, hot isostatic pressing is performed for 360 min at 180 MPa and 1300°C to obtain a pure titanium aluminum alloy target.
[0066] Example 4
[0067] This embodiment provides a method for recycling a titanium aluminum alloy target material. The recycling method is different from that of Embodiment 1 only in that:
[0068] In this embodiment, the hydrofluoric acid used in the pickling in step (2) is replaced with nitric acid in an equal molar amount, so that the acid solution is adjusted to nitric acid and water.
[0069] Example 5
[0070] This embodiment provides a method for recycling a titanium aluminum alloy target material. The recycling method is different from that of Embodiment 1 only in that:
[0071] In this embodiment, the amount of high-purity aluminum particles added in step (3) is adjusted to 0.6 wt % of the mass of the target block without impurities.
[0072] Example 6
[0073] This embodiment provides a method for recycling a titanium aluminum alloy target material. The recycling method is different from that of Embodiment 1 only in that:
[0074] In this embodiment, the amount of high-purity aluminum particles added in step (3) is adjusted to 1 wt% of the mass of the target block without impurities.
[0075] Example 7
[0076] This embodiment provides a method for recycling a titanium aluminum alloy target material. The recycling method is different from that of Embodiment 1 only in that:
[0077] In this embodiment, the temperature of the vacuum suspension smelting in step (3) is adjusted to 1450°C.
[0078] Example 8
[0079] This embodiment provides a method for recycling a titanium aluminum alloy target material. The recycling method is different from that of Embodiment 1 only in that:
[0080] In this embodiment, the temperature of the vacuum suspension smelting in step (3) is adjusted to 1580°C.
[0081] Example 9
[0082] This embodiment provides a method for recycling a titanium aluminum alloy target material. The recycling method is different from that of Embodiment 1 only in that:
[0083] In this embodiment, the temperature of the hot isostatic pressing in step (3) is adjusted to 1200°C.
[0084] Example 10
[0085] This embodiment provides a method for recycling a titanium aluminum alloy target material. The recycling method is different from that of Embodiment 1 only in that:
[0086] In this embodiment, the temperature of the hot isostatic pressing in step (3) is adjusted to 1350°C.
[0087] Embodiment 11
[0088] This embodiment provides a method for recycling a titanium aluminum alloy target material. The recycling method is different from that of Embodiment 1 only in that:
[0089] In this embodiment, the pressure of the hot isostatic pressing in step (3) is adjusted to 140 MPa.
[0090] Example 12
[0091] This embodiment provides a method for recycling a titanium aluminum alloy target material. The recycling method is different from that of Embodiment 1 only in that:
[0092] In this embodiment, the hot isostatic pressing pressure in step (3) is adjusted to 190 MPa.
[0093] Comparative Example 1
[0094] This comparative example provides a method for recycling a titanium aluminum alloy target material. The difference between the recycling method and Example 1 is that:
[0095] In this comparative example, the hot isostatic pressing described in step (3) was omitted.
[0096] Comparative Example 2
[0097] This comparative example provides a method for recycling a titanium aluminum alloy target material. The difference between the recycling method and Example 1 is that:
[0098] In this comparative example, the vacuum suspension melting described in step (3) is adjusted to electromagnetic induction melting; the temperature of the electromagnetic induction melting is 1250°C.
[0099] Comparative Example 3
[0100] This comparative example provides a method for recycling a titanium aluminum alloy target material. The difference between the recycling method and Example 1 is that:
[0101] In this comparative example, the casting and hot isostatic pressing in step (3) are adjusted to ultrasonic treatment and cooling in an oxygen-free environment; the frequency of the ultrasonic treatment is 25 kHz.
[0102] Comparative Example 4
[0103] This comparative example provides a method for recycling a titanium aluminum alloy target material. The difference between the recycling method and Example 1 is that:
[0104] In this comparative example, the mixing process described in step (3) was omitted.
[0105] Performance testing:
[0106] (1) The purity of the titanium aluminum alloy target materials provided in the above embodiments and comparative examples was tested by glow discharge mass spectrometry, and the results are shown in Table 1;
[0107] (2) The internal defect rate of the titanium aluminum alloy target provided in the above embodiment and comparative example was measured by an ultrasonic scanner, and the results are shown in Table 1;
[0108] (3) The internal structure of the titanium-aluminum alloy target provided in the above embodiment and comparative example was observed using a scanning electron microscope. The results are shown in Table 1.
[0109] Table 1
[0110] purity / % Target internal defect rate / % Organizational Structure Example 1 99.995 0 Single γ phase structure Example 2 99.995 0 Single γ phase structure Example 3 99.995 0 Single γ phase structure Example 4 99.9 0 Single γ phase structure Example 5 99.995 0 <![CDATA[α2 + γ phase]]> Example 6 99.995 0 <![CDATA[β0 + γ phase]]> Example 7 99.9 1 Single γ phase structure Example 8 99.995 0 <![CDATA[α2+γ phase]]> Example 9 99.995 2 <![CDATA[α2+γ duplex structure]]> Example 10 99.995 0 <![CDATA[α2 + γ duplex structure]]> Embodiment 11 99.995 5 Single γ phase structure Comparative Example 1 99.995 5 <![CDATA[α2+γ duplex structure]]> Comparative Example 2 99.95 0 Single γ phase structure Comparative Example 3 99.995 5 <![CDATA[α2 + γ duplex structure]]> Comparative Example 4 99.995 0 <![CDATA[β0 + γ phase]]>
[0111] From the data in Table 1, we can see the following points:
[0112] (1) Comprehensive analysis of Examples 1-3 shows that the method provided by the present invention can realize the recycling of titanium aluminum alloy residual targets, and obtain titanium aluminum alloy targets with high purity, uniform composition and structure, which can be used again in the sputtering process;
[0113] (2) Comprehensive analysis of Example 1 and Examples 5-6 shows that adding an appropriate amount of high-purity aluminum particles before smelting is beneficial to replenishing the aluminum burnout during the smelting process; if the amount of addition is too much or too little, β0 or α2 phases will be generated, resulting in uneven internal structure of the target material;
[0114] (3) Comprehensive analysis of Example 1 and Examples 7-8 shows that lowering the temperature of vacuum levitation melting will lead to reduced purity of the target material and internal defects; increasing the temperature of vacuum levitation melting will cause serious burnout of the alloy material, affect the internal structure of the organization, and cause the problem of uneven internal organization of the target material; thus, it is shown that the regulation of the vacuum levitation melting temperature is an important factor in effectively controlling the purity and uniformity of the target material;
[0115] (4) Comprehensive analysis of Example 1, Examples 9-11 and Comparative Example 1 shows that, due to the unreasonable selection of the hot isostatic pressing temperature range of Examples 9-10, the unreasonable selection of the hot isostatic pressing pressure range of Example 11, and the fact that hot isostatic pressing was not performed on the comparative example, defects and / or uneven internal structure appeared inside the obtained target material, which indicates that the temperature and pressure of hot isostatic pressing are important factors for effectively controlling the internal structure of the target material;
[0116] (5) Comprehensive analysis of Example 1 and Comparative Example 2 shows that, compared with the vacuum suspension melting method adopted by the present invention, the use of the crucible in the electromagnetic induction melting process introduces impurities, which reduces the purity of the obtained target material;
[0117] (6) Comprehensive analysis of Example 1 and Comparative Example 3 shows that, compared with the present invention, ultrasonic treatment and cooling cannot achieve the effects of densification, structural transformation and homogenization of the material.
[0118] In summary, the method for recycling titanium-aluminum alloy targets provided by the present invention obtains titanium-aluminum alloy targets with high purity, uniform composition and structure by vacuum suspension melting of titanium-aluminum alloy residual targets and hot isostatic pressing of target blanks. This method has a short production cycle and high efficiency, which is conducive to large-scale promotion and application.
[0119] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A method for recycling titanium aluminum alloy target material, characterized in that: The recycling method comprises the following steps: (1) pretreating a titanium-aluminum alloy residual target to obtain a titanium-aluminum alloy target block; (2) sequentially pickling, water washing, organic solvent cleaning and vacuum drying the titanium aluminum alloy target block obtained in step (1) to obtain a decontaminated target block; (3) The impurity-removed target block obtained in step (2) is sequentially subjected to mixing, vacuum suspension melting, casting and hot isostatic pressing to obtain the titanium-aluminum alloy target material.
2. The recycling method according to claim 1, characterized in that: The aluminum element accounts for 35-37 wt % in the titanium-aluminum alloy residual target in step (1).
3. The recycling method according to claim 1 or 2, characterized in that: The pre-processing includes a turning process and a segmentation process performed in sequence; Preferably, the turning process is to remove the backing plate and the sputtering layer on the surface of the titanium aluminum alloy residual target; Preferably, the segmentation process is to make the length, width and thickness of the titanium aluminum alloy target block all be 20 to 40 mm.
4. The recycling method according to any one of claims 1 to 3, characterized in that: The acid solution used for pickling in step (2) is composed of nitric acid, hydrofluoric acid and water in a molar ratio of 1 to 2:1:4.5 to 5.5; Preferably, the pickling time is 15 to 30 minutes; Preferably, the organic solvent in the organic solvent cleaning in step (2) comprises any one of isopropanol, acetone or ethanol, or a combination of at least two thereof; Preferably, the organic solvent cleaning time in step (2) is 10 to 15 minutes; Preferably, the organic solvent cleaning in step (2) is carried out under ultrasonic conditions.
5. The recycling method according to any one of claims 1 to 4, characterized in that: The vacuum drying temperature in step (2) is 100-150° C. Preferably, the vacuum drying time in step (2) is 2 to 3 hours; Preferably, the vacuum drying in step (2) further includes a cooling treatment.
6. The recycling method according to any one of claims 1 to 5, characterized in that: The mixed material in step (3) includes mixing high-purity aluminum particles and the impurity-removed target block obtained in step (2); Preferably, the addition amount of the high-purity aluminum particles is 0.7-0.8wt% of the mass of the impurity-removing target block; Preferably, the purity of the high-purity aluminum particles is ≥99.999%.
7. The recycling method according to any one of claims 1 to 6, characterized in that: The vacuum degree of the vacuum suspension smelting in step (3) is ≤0.05 Pa; Preferably, the temperature of the vacuum suspension smelting in step (3) is 1500-1550°C; Preferably, the vacuum suspension smelting time in step (3) is 15 to 30 minutes.
8. The recycling method according to any one of claims 1 to 7, characterized in that: The hot isostatic pressing pressure in step (3) is 150-180 MPa; Preferably, the temperature of the hot isostatic pressing in step (3) is 1250-1300°C; Preferably, the hot isostatic pressing time in step (3) is 240 to 360 minutes.
9. The recycling method according to any one of claims 1 to 8, characterized in that: The purity of the titanium aluminum alloy target material is greater than 99.99%; Preferably, the titanium aluminum alloy target has a single γ phase.
10. The recycling method according to any one of claims 1 to 9, characterized in that: The recycling method comprises the following steps: (1) turning a titanium-aluminum alloy residual target in which the aluminum element accounts for 35 to 37 wt % to remove a back plate and a sputtering layer on the surface of the titanium-aluminum alloy residual target, and then cutting the target to obtain a titanium-aluminum alloy target block having a length, width and thickness of 20 to 40 mm; (2) The titanium aluminum alloy target block obtained in step (1) is sequentially pickled with an acid solution composed of nitric acid, hydrofluoric acid and water in a molar ratio of 1 to 2:1:4.5 to 5.5 for 15 to 30 minutes, washed with water, and cleaned with an organic solvent in an ultrasonic wave for 10 to 15 minutes, vacuum dried at 100 to 150° C. for 2 to 3 hours, and then cooled to obtain a de-impurified target block; (3) High-purity aluminum particles with an addition amount of 0.7-0.8 wt% of the mass of the impurity-removed target block and the impurity-removed target block obtained in step (2) are mixed, and then vacuum suspension melting is performed for 15-30 min at a vacuum degree of ≤0.05 Pa and 1500-1550° C. After casting, hot isostatic pressing is performed for 240-360 min at 150-180 MPa and 1250-1300° C. to obtain a titanium aluminum alloy target with a purity of >99.99% and a single γ phase.
Citation Information
Patent Citations
Preparation method of titanium-aluminum alloy target material
CN112725658A
Aluminum-scandium alloy target material and preparation method thereof
CN114774865A