CVD method and system
By combining static and dynamic methods in CVD growth, the removal speed of the substrate is adjusted to compensate for gas loss, and the problem of poor uniformity in CVD growth is solved, achieving high-efficiency uniform growth effect.
Patent Information
- Application Number
- CN202411045439.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-08
Smart Images

Figure CN118910593A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of preparing thin films or coatings by using chemical vapor deposition (CVD), and in particular to a preparation technology for improving CVD growth uniformity and preparation efficiency. Background Art
[0002] The air inlet and outlet of a tubular vacuum high-temperature growth furnace are generally located at the two ends of the furnace body. During CVD growth, the reaction gas enters from the air inlet and the waste gas after the reaction is discharged from the air outlet. Therefore, along the flow direction of the reaction gas, the reaction gas gradually reacts and is consumed as it flows through the high-temperature zone, causing the CVD growth rate at various locations in the process chamber to gradually decrease along the gas flow direction, resulting in large differences in the surface uniformity of the final product.
[0003] Taking the preparation of graphene by CVD as an example, graphene is a material with excellent mechanical, optical and electrical properties. At present, in the preparation method of graphene, the process of manufacturing graphene conductive fabric by CVD method using a tubular vacuum high-temperature growth furnace usually adopts a static growth process, such as Figure 2 As shown in FIG. 1 , after placing a substrate such as glass fiber cloth in the CVD growth zone, the temperature is raised to the process temperature and then a carbon source is introduced. After a certain period of time, the introduction of the carbon source is stopped, the temperature is lowered, and then the glass fiber cloth and other substrates are taken out. In this method, the carbon source is gradually consumed as it flows through the high-temperature growth zone, resulting in a gradual decrease in the CVD growth rate at various locations in the CVD growth zone along the gas flow direction, and the surface uniformity of the final product is quite different. In order to solve the problem of product surface uniformity, one approach is to adopt a roll-to-roll dynamic growth method, such as Figure 3 As shown, the roll located in the sample placement chamber is placed, and the roll located in the sample collection chamber is collected synchronously, so that the glass fiber cloth passes through the entire high-temperature growth zone at a uniform speed, thereby ensuring that the surface uniformity of the product is close to uniform. For example, Chinese patent application document CN104988471A discloses a rapid cooling roll-to-roll plasma enhanced CVD continuous growth furnace. The above-disclosed technical solution uses a roll-to-roll dynamic growth method, but this method is limited by the inner diameter of the quartz tube and can only be applied to small and wide glass fiber cloths. In addition, the CVD growth speed is slow, time-consuming, and the efficiency is low.
[0004] Therefore, there is an urgent need to study a CVD preparation technology that can achieve uniform CVD growth while maintaining high preparation efficiency. Summary of the invention
[0005] In the process of CVD growth in a tubular vacuum high-temperature growth furnace, the reaction gas is gradually consumed as it flows through the high-temperature zone, causing the CVD growth rate in each part of the CVD growth zone to gradually decrease along the gas flow direction, resulting in a large difference in the surface uniformity of the final product. To address this problem, the present invention adopts a combination of static and dynamic methods, first allowing the substrate as a whole to undergo CVD growth in the CVD growth zone, and after a certain period of time, dragging the substrate out of the CVD zone at a certain speed in the reverse direction of the gas flow, so that the area with a fast growth rate ends growth first, and the area with a slow growth rate grows for a longer time, thereby greatly improving the uniformity of the product surface.
[0006] In view of the above-mentioned limitations, the present invention proposes a CVD method and system.
[0007] A CVD method comprising the following steps:
[0008] Step (1): placing a substrate material in a CVD growth zone, heating it to a first temperature, and then introducing a reaction gas, wherein the reaction gas flows from one end of the CVD growth zone to the other end, and starting CVD growth;
[0009] Step (2): after a static growth time, the substrate material is moved out of the CVD growth zone at a preset speed in a direction opposite to the flow direction of the reaction gas;
[0010] Step (3): All substrate materials are moved out of the CVD growth area, and the CVD growth is completed.
[0011] Further: the preset speed is a dynamic moving speed, and the dynamic moving speed is:
[0012]
[0013] Among them, A is the growth rate at the starting point of the growth zone, B is the growth rate at the end point of the growth zone, L is the length of the CVD growth zone, and t is the static growth time.
[0014] Furthermore: the substrate material is in a planar shape, or is rolled into a roll; the axial direction of the substrate material rolled into a roll is parallel to the flow direction of the reaction gas.
[0015] Furthermore: the reaction gas enters the CVD growth zone from a distance greater than or equal to 0.2 meters from the starting point of the growth zone.
[0016] Furthermore: the substrate material is high temperature resistant fiber cloth or metal foil, and the reaction gas is a carbon source gas, which is used to deposit graphene on the surface of the substrate material.
[0017] Furthermore: the length of the CVD growth zone is 1.0-2.0 meters, the first temperature is 500-1200° C., the flow rate of the carbon source gas is 200-2000 standard milliliters per minute, and the static growth time is 50-500 minutes.
[0018] A CVD system comprises: a lofting chamber: the substrate material is lofted from the lofting chamber;
[0019] Transmission device: the transmission device delivers the substrate material into or out of the CVD growth area;
[0020] CVD growth zone: in the CVD growth zone, a thin film or coating is grown using a CVD method;
[0021] An air inlet device and an air outlet device: the air inlet device and the air outlet device are respectively located on two sides of the CVD growth area;
[0022] The CVD system uses the CVD method to prepare a thin film or a coating.
[0023] Furthermore: the transmission device includes a lofting belt and a transmission mechanism, the transmission mechanism drives the lofting belt to move between the lofting chamber and the CVD growth zone, the substrate material is placed on the lofting belt, and the transmission mechanism drives the lofting belt to send the substrate material into or out of the CVD growth zone.
[0024] Furthermore: a heating device, an air inlet, and an air outlet are arranged in the CVD growth zone, the reaction gas flows in from the air inlet and flows out from the air outlet; and the air outlet device is arranged at the rear end of the air outlet.
[0025] Furthermore, the air intake device is an air intake pipe, the reaction gas enters the air inlet from the air intake pipe, and the distance between the air intake pipe and the starting point of the growth zone is greater than or equal to 0.2 meters. Compared with the related art, the present invention has the following advantages:
[0026] The CVD preparation method provided in the first aspect of the present invention adopts a combination of static and dynamic methods to prepare thin films. Compared with the static growth method, the uniformity of the product surface can be greatly improved. Compared with the dynamic growth method, the growth on a wide substrate material can be achieved and the growth efficiency is greatly improved.
[0027] The CVD preparation system provided in the second aspect of the present invention adopts a combination of static and dynamic methods to prepare thin films due to the provision of a sample chamber and a transmission device. Compared with the static growth method, the uniformity of the product surface can be greatly improved, and compared with the dynamic growth method, the growth on a wide substrate material can be achieved, and the growth efficiency is greatly improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 A schematic diagram of the structure of a CVD system according to an embodiment of the present invention;
[0029] Figure 2 A schematic diagram of the structure of a static CVD system of the related art;
[0030] Figure 3 It is a structural schematic diagram of a dynamic CVD system of related technology.
[0031] Description of reference numerals:
[0032] 10-Lofting cavity
[0033] 20-CVD growth area
[0034] 21- Transmission
[0035] 22-Intake pipe
[0036] 23- Exhaust device
[0037] 30-Substrate material DETAILED DESCRIPTION
[0038] In order to make the purpose, technical solution and advantages of the present invention more clear, the present invention is further described in detail below. However, it should be understood that the description herein is only used to explain the present invention and is not used to limit the scope of the present invention.
[0039] Unless otherwise defined, all technical terms and scientific terms used herein have the same meanings as those generally understood by those skilled in the art of the present invention. The terms used in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The characterization means involved in this article can refer to the relevant descriptions in the prior art and will not be repeated herein.
[0040] In order to further understand the present invention, the present invention is further described in detail below in conjunction with the best embodiment.
[0041] A CVD preparation method comprises the following steps:
[0042] Step (1): placing the substrate material 30 in the CVD growth zone 20, heating it to a first temperature, and then introducing a reaction gas, wherein the reaction gas flows from one end of the CVD growth zone to the other end, and starting CVD growth;
[0043] Step (2): after the static growth time, the substrate material 30 is moved out of the CVD growth zone 20 at a preset speed in the opposite direction of the reaction gas flow direction;
[0044] Step (3): All substrate materials 30 are moved out of the CVD growth area 20, and the CVD growth is completed.
[0045] CVD (Chemical Vapor Deposition) is a technology that converts gaseous reactants into solid materials at high temperatures and deposits them on the surface of substrate materials to form thin films or coatings. The basic process of CVD generally includes steps such as gas delivery, chemical reaction and deposition. Reaction temperature, reaction gas ratio and reaction kinetics are all key factors affecting the quality and efficiency of CVD products.
[0046] Furthermore: the preset speed is a dynamic moving speed, and the dynamic moving speed is:
[0047]
[0048] Wherein, A is the growth rate of the starting point of the growth zone, B is the growth rate of the ending point of the growth zone, L is the length of the CVD growth zone (20) (the length from the starting point of the growth zone to the ending point of the growth zone), and t is the static growth time; the starting point of the growth zone refers to the point where the CVD growth zone 20 is closest to the air inlet, and the shape of the air inlet can adopt the common CVD growth zone air inlet shape. The air inlet can be a planar shape, such as a circle, square, rectangle, polygon, etc. The present invention is not limited to the above shapes, as long as the shape of the air inlet does not affect the air intake effect required for the CVD reaction. When the air inlet is a planar shape, the plane is perpendicular to the flow direction of the reaction gas, so all the starting points of the growth zones can be located on a plane, and the plane is parallel to the air inlet plane; the ending point of the growth zone refers to the point where the CVD growth zone 20 is farthest from the air inlet, and all the ending points of the growth zones are located on a plane, and the plane is parallel to the air inlet plane.
[0049] The CVD growth rate is affected by the concentration of the reaction gas. Along the flow direction of the reaction gas, the reaction gas is gradually consumed as it flows through the CVD growth zone 20. The CVD growth rate at various locations in the CVD growth zone 20 gradually decreases along the gas flow direction. According to theoretical calculations (see Table 1 and Table 2) and experimental verification (see Example 1), moving the substrate material 30 at the dynamic moving speed calculated by Formula 1 can compensate for the decrease in growth rate caused by the gradual consumption of the reaction gas, thereby improving the uniformity of the film or coating.
[0050] like Figure 1 As shown, the reaction gas flows in a direction from the gas inlet to the gas outlet of the CVD growth zone 20 (the direction of the arrow in the figure), and the change in the number of arrows indicates that the concentration of the reaction gas gradually decreases along this direction.
[0051] Furthermore: the substrate material 30 is in a planar shape, or is wound into a roll; the axial direction of the substrate material 30 wound into a roll is parallel to the flow direction of the reaction gas.
[0052] Preferably, the substrate material 30 is wound into a roll. By winding the planar substrate material into a roll, a large-sized film can be prepared at one time, effectively improving the preparation efficiency.
[0053] Further: the reaction gas enters the CVD growth zone 20 from a distance greater than or equal to 0.2 meters from the starting point of the growth zone, for example, 0.2 meters, 0.3 meters, 0.4 meters, 0.5 meters, etc. from the starting point of the growth zone. The present invention is not limited to the listed values, and other unlisted values are also applicable. Through this setting, the flow distance of the reaction gas before entering the growth zone is increased, so that the flow rate of the reaction gas is more uniform.
[0054] Furthermore, the substrate material 30 is a high temperature resistant fiber cloth or a metal foil, and the reaction gas is a carbon source gas, which is used to deposit graphene on the surface of the substrate material 30 .
[0055] Preferably, the high temperature resistant fiber cloth is glass fiber cloth, alumina fiber cloth, or basalt fiber cloth.
[0056] For the high temperature resistant fiber cloth, it is woven from fibers and has a porous structure, so the carbon source gas flow can pass through the rolled fiber cloth unimpeded; for the metal foil, it is a dense layered foil, and each layer should maintain a certain distance when winding, so that the carbon source gas flow can flow unimpeded along the axial direction of the rolled substrate.
[0057] Furthermore: the length of the CVD growth zone 20 is directly related to the size of the heating zone of the CVD equipment, and when the CVD growth zone is longer, the concentration of the reaction gas decreases more significantly along the gas flow direction, and the better it can reflect the excellent uniformity of the preparation method of the present invention. The present invention does not specifically limit the length of the CVD growth zone 20, as long as it can meet the CVD growth conditions.
[0058] Specifically for the CVD preparation of graphene, the common CVD growth zone 20 length is 1.0-2.0 meters, for example, the CVD growth zone 20 length is 1.0 meters, 1.1 meters, 1.2 meters, 1.3 meters, 1.4 meters, 1.5 meters, 1.6 meters, 1.7 meters, 1.8 meters, 1.9 meters, 2.0 meters, but the present invention is not limited to the listed values;
[0059] The first temperature is 500-1200° C., for example, the first temperature is 500° C., 600° C., 700° C., 800° C., 900° C., 1000° C., 1100° C., 1200° C., but the present invention is not limited to the listed values, and other values not listed are also applicable;
[0060] The static growth time is 50-500 minutes, for example, the static growth time is 50 minutes, 100 minutes, 150 minutes, 200 minutes, 300 minutes, 400 minutes, 500 minutes, but the present invention is not limited to the listed values, and other unlisted values are equally applicable.
[0061] Further: the flow rate of the carbon source gas is 200-2000 standard milliliters per minute (sccm), for example, the flow rate of the carbon source gas is 200 sccm, 500 sccm, 1000 sccm, 2000 sccm; the present invention is not limited to the listed values, and other values not listed are also applicable;
[0062] like Figure 1 As shown, a CVD preparation system comprises:
[0063] Lofting cavity 10: the substrate material 30 is lofted from the lofting cavity 10;
[0064] Transmission device 21: the transmission device 21 delivers the substrate material 30 into or out of the CVD growth area 20;
[0065] CVD growth zone 20: In the CVD growth zone 20, a thin film or coating is grown using a CVD method;
[0066] Air inlet device and air outlet device 23: the air inlet device and air outlet device 23 are respectively located on both sides of the CVD growth area;
[0067] The CVD system uses the CVD method for preparing graphene to prepare a film or a coating.
[0068] The gas inlet device is used to introduce reaction gas into the CVD growth area 20, and the gas outlet device 23 is used to discharge the remaining reaction gas from the CVD growth area 20, so as to control the flow rate of the reaction gas and the concentration of the reaction gas.
[0069] Further: the transmission device 21 includes a lofting belt and a transmission mechanism, the transmission mechanism drives the lofting belt to move between the lofting chamber 10 and the CVD growth area 20, and the substrate material 30 is placed on the lofting belt;
[0070] The transmission mechanism drives the lofting belt to deliver the substrate material 30 into or out of the CVD growth zone 20 .
[0071] In step (1), when the substrate material 30 is laid out, the amount of the substrate material 30 for the primary graphene growth is fed into the CVD growth zone 20 by the transmission device. The amount of the planar substrate material 30 for the primary graphene growth can be less than or equal to the area of the CVD growth zone 20, preferably equal to the area of the CVD growth zone 20, or the axial length of the roll-shaped substrate material 30 for the primary graphene growth can be less than or equal to the length of the CVD growth zone 20, preferably equal to the length of the CVD growth zone 20, so as to maximize the preparation efficiency.
[0072] Furthermore, a heating device, an air inlet, and an air outlet are provided in the CVD growth area 20, and the reaction gas flows in from the air inlet and flows out from the air outlet; and the air outlet device 23 is provided at the rear end of the air outlet. The air outlet device 23 can control the flow rate of the reaction gas and the concentration of the reaction gas.
[0073] Further: the air intake device is an air intake pipe 22, the reaction gas enters the air inlet from the air intake pipe 22, and the distance between the air intake pipe 22 and the starting point of the growth zone is greater than or equal to 0.2 meters, such as 0.2 meters, 0.3 meters, 0.4 meters, 0.5 meters, etc. The present invention is not limited to the listed values, and other values not listed in the numerical range are also applicable. A plurality of air outlet holes or air outlet slits are provided on the air intake pipe 22 at equal intervals to transport the reaction gas to the air inlet of the CVD growth zone 20. The air intake pipe can be an annular structure, or it can be one or more mutually parallel, horizontally placed or vertically placed elongated structures. The present invention is not limited to the above structures, as long as it does not affect the air intake effect of the reaction gas in the CVD method of the present invention.
[0074] The following uses CVD to prepare graphene as an example, and according to the theoretical principle of CVD thin film preparation, the technical effect of the present invention is derived by theoretical calculation. It can be understood that according to the CVD preparation principle, the following theoretical calculation can be extended to the case of CVD method to prepare thin films or coatings of other materials.
[0075] Table 1 is the theoretical calculation results of the graphene product prepared by the method of the present invention. The discrete coefficient of the "total thickness" is 0.326, and the discrete coefficient of the static growth graphene thickness ("static growth thickness") is 4.474. The above results show that the method of combining static and dynamic growth of the present invention can effectively improve the uniformity;
[0076] Coefficient of dispersion C v The calculation formula of (coefficient of variat ion) is:
[0077]
[0078] Wherein, σ is the standard deviation of graphene thickness, and μ is the average graphene thickness.
[0079] Table 1
[0080]
[0081] Table 2 shows the theoretical calculation results of the graphene product prepared by calculating the dynamic moving speed by selecting the growth rate at the middle point during calculation (calculated only to the middle point). The total thickness dispersion coefficient (0.317) is much smaller than the dispersion coefficient (2.223) of the static preparation method within the range from the starting point to the middle point (see Table 2 "Static Growth Thickness"), which greatly improves the uniformity of the thickness. However, compared with the case of selecting the end point of the growth zone to calculate the dynamic moving speed in Table 1, the dispersion coefficient of the total thickness within the same distance from the starting point of the growth zone in Table 1 (within the range of 100-700, thick frame in Table 1) is only 0.091, indicating that selecting the end point of the CVD growth zone as the calculation point of the dynamic moving speed is the best solution. The middle point refers to the middle point between the starting point of the growth zone and the end point of the growth zone in Table 1, that is, the middle point located in the CVD growth zone.
[0082] Table 2
[0083]
[0084] In Table 1 and Table 2, the length (distance) unit is millimeter, the thickness unit is micrometer, the time unit is second, and the speed unit is micrometer / second. It can be understood that the above units are only calculation examples, and the present invention is not limited to the above specific units, and consistent units can be selected.
[0085] The present invention and the technical effects of the present invention are further described in detail below with specific experiments (Example 1, Comparative Example 1).
[0086] Example 1
[0087] Select 0.1mm thick glass fiber cloth, 7 meters in length and 700mm in width, roll it into a cloth roll (outer diameter is about 50mm), the heating zone of the tubular vacuum high temperature growth furnace is 2 meters, the length of the CVD growth zone is 1.4 meters, the first temperature is 850℃, the pressure is 1000 Pa, the carbon source flow rate is 1800sccm, and it is placed 0.1 meters away from the air inlet of the growth zone. Figure 1 shown.
[0088] Take the following process steps:
[0089] 1. After placing the glass fiber cloth in the CVD growth zone 20, the temperature is raised to a first temperature, and then a carbon source is introduced to start CVD growth;
[0090] 2. After the static growth time, the transmission device 21 is started to move the glass fiber cloth out of the growth zone in the reverse direction of the air flow at a dynamic moving speed;
[0091] 3. Stop introducing the carbon source, cool down, and then take out the glass fiber cloth.
[0092] From formula 1, we can deduce:
[0093]
[0094] Using static growth for 60 minutes, the experimental measurement of B / A = 0.6, so the dynamic moving speed is calculated to be 46.7 mm / min, and the total time is 60+800 / 46.7 = 77 minutes.
[0095] After the growth is completed, the surface resistance distribution is measured as follows:
[0096] Table 3
[0097] Location 10cm 20cm 30cm 40cm 50cm 60cm 70cm Coefficient of dispersion Sheet resistance 794 786 771 757 753 803 796 2.5%
[0098] Since the actual CVD growth process has more influencing factors than the theoretical calculations in Tables 1 and 2, the discrete coefficients in Table 3 are not completely consistent with the corresponding values in Tables 1 and 2. However, compared with the discrete coefficients in Comparative Example 1, the surface uniformity of the product of the present invention is greatly improved.
[0099] Comparative Example 1: Static Growth
[0100] The other conditions are the same as those in the embodiment, except that the static growth is only performed for 70 minutes. After the growth is completed, the surface resistance distribution is measured as follows:
[0101] Table 6
[0102] Location 10cm 20cm 30cm 40cm 50cm 60cm 70cm Coefficient of dispersion Sheet resistance 729 746 755 765 784 861 877 7.3%
[0103] Comparison results show that the thickness dispersion coefficient of graphene produced by the method of the present invention is reduced from 7.3% of the static method to 2.5%, which significantly improves the uniformity of the product surface.
[0104] Comparative Example 2: Dynamic growth in a cloth roll
[0105] The other conditions are the same as those in Example 1, except that dynamic growth is adopted with a speed of 17.8 mm / min.
[0106] The total time is (1400+700) / 17.8=118 minutes. 700 mm is the width of the cloth roll, and 1400 mm is the length of the CVD growth zone.
[0107] Comparative results show that the total time consumption of the present invention is 77 minutes, which can save a lot of time compared with dynamic growth and greatly improve the preparation efficiency.
[0108] In an embodiment of the present invention, the CVD method and system of the present invention are used to prepare graphene. It can be understood that, based on the preparation principle of CVD, it can be inferred that the method and system are not limited to the above-mentioned applications, but can also be used in all CVD preparation technologies applicable to the inventive concept of the present invention.
[0109] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modification, equivalent substitution or improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A CVD method, characterized in that: The following steps are involved: Step (1): placing a substrate material (30) in a CVD growth zone (20), heating it to a first temperature, and then introducing a reaction gas, wherein the reaction gas flows from one end of the CVD growth zone to the other end, and starting CVD growth; Step (2): after a static growth time, the substrate material (30) is moved out of the CVD growth zone (20) at a preset speed in a direction opposite to the flow direction of the reaction gas; Step (3): All substrate materials (30) are moved out of the CVD growth area (20), and the CVD growth is terminated.
2. The method according to claim 1, characterized in that: The preset speed is a dynamic moving speed, and the dynamic moving speed is: Wherein, A is the growth rate at the starting point of the growth zone, B is the growth rate at the end point of the growth zone, L is the length of the CVD growth zone (20), and t is the static growth time.
3. The method according to claim 1, characterized in that: The substrate material (30) is in a planar shape, or is wound into a roll; the axial direction of the substrate material (30) wound into a roll is parallel to the flow direction of the reaction gas.
4. The method according to claim 1, characterized in that: The reaction gas enters the CVD growth zone (20) from a point greater than or equal to 0.2 meters away from the starting point of the growth zone.
5. The method according to any one of claims 1 to 4, characterized in that: The substrate material (30) is a high temperature resistant fiber cloth or a metal foil, and the reaction gas is a carbon source gas, which is used to deposit graphene on the surface of the substrate material (30).
6. The method according to claim 5, characterized in that: The length of the CVD growth zone (20) is 1.0-2.0 meters, the first temperature is 500-1200° C., the flow rate of the carbon source gas is 200-2000 standard milliliters per minute, and the static growth time is 50-500 minutes.
7. A CVD system, characterized in that: include: A lofting cavity (10): the substrate material (30) is lofted from the lofting cavity (10); Transmission device (21): the transmission device (21) transports the substrate material (30) into or out of the CVD growth zone (20); CVD growth zone (20): a thin film or coating is grown using a CVD method in the CVD growth zone (20); An air inlet device and an air outlet device (23): the air inlet device and the air outlet device (23) are respectively located on two sides of the CVD growth area; The CVD system uses the method according to any one of claims 1 to 6 to prepare a thin film or a coating.
8. The system according to claim 7, characterized in that: The transmission device (21) comprises a lofting belt and a transmission mechanism, wherein the transmission mechanism drives the lofting belt to move between the lofting chamber (10) and the CVD growth zone (20), the substrate material (30) is placed on the lofting belt, and the transmission mechanism drives the lofting belt to send the substrate material (30) into or out of the CVD growth zone (20).
9. The system according to claim 7, characterized in that: A heating device, an air inlet, and an air outlet are arranged in the CVD growth area (20); the reaction gas flows in from the air inlet and flows out from the air outlet; and the air outlet device (23) is arranged at the rear end of the air outlet.
10. The system according to claim 9, characterized in that: The air intake device is an air intake pipe (22), the reaction gas enters the air inlet from the air intake pipe (22), and the distance between the air intake pipe (22) and the starting point of the growth zone is greater than or equal to 0.2 meters.
Citation Information
Cited By
Roll-to-roll CVD (Chemical Vapor Deposition) production equipment and process
CN120158734A