Preparation method of solution formula for laser-induced liquid phase deposition copper plating, solution formula and copper plating method

By using the formula of copper salt, chelating agent, reducing agent, stabilizer and nanocopper powder in laser-induced copper depositing technology, combined with a protective film containing hydroxyl polymer compounds, the looseness of copper deposited layer and solution corrosion in the prior art is solved. The high-quality, stable and environmentally friendly copper plating layer deposition is achieved, reducing production costs and environmental impact.

CN118910596AActive Publication Date: 2024-11-08GUANGDONG UNIV OF TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410826026.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-25
Publication Date
2024-11-08
Estimated Expiration
2044-06-25

AI Technical Summary

Technical Problem

The solution formula in the existing laser-induced copper depositing technology has side reactions during the reaction process, resulting in loose and rough copper deposited layer and poor binding force. The chemical components in the solution are corrosive and toxic, which affects operation safety and environment, and waste liquid The processing is complex and costly.

Method used

Using the formula of copper salt, chelating agent, reducing agent, stabilizer, hydroxyl-containing polymer compounds and nano-copper powder, a laser-induced liquid deposition solution is formed by adding nano-copper powder to Promote uniform deposition and use hydroxyl-containing polymer compounds to form a protective film to inhibit oxidation reaction.

Benefits of technology

It achieves the improvement of high quality, stability and service life of copper plating layers, reduces the generation of holes and cracks, ensures the consistency of the plate surface, reduces the impact on operators and the environment, and simplifies waste liquid treatment. Reduced production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910596A_ABST
    Figure CN118910596A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of copper plating, in particular to a preparation method of a solution formula for laser-induced liquid phase deposition copper plating, the solution formula and a copper plating method. The preparation method comprises the following steps: S1, respectively dissolving a copper salt and a chelating agent with deionized water to obtain a copper salt solution and a chelating agent solution, and mixing the copper salt solution and the chelating agent solution to obtain a transparent blue first mixed solution; s2, sequentially adding a reducing agent and a stabilizer into the first mixed solution, and uniformly mixing to obtain a second mixed solution; s3, an alkaline reagent is added into the second mixed solution, the pH of the second mixed solution is adjusted to be alkaline, and a third mixed solution serving as a copper ion solution system is obtained; and S4, a hydroxyl-containing high-molecular compound is added into the third mixed solution, nano copper powder is added after even mixing, even mixing is conducted again, and the solution formula for laser-induced liquid phase deposition copper plating is obtained and has the advantages of being environmentally friendly and stable and even in deposition process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of copper plating, and in particular to a preparation method of a solution formula for laser-induced liquid phase deposition copper plating, a solution formula and a copper plating method. Background Art

[0002] In the modern electronics manufacturing industry, laser-induced copper deposition technology has become an important process in the manufacture of printed circuit boards (PCBs), semiconductor packaging and microelectronic devices due to its advantages of high precision and high resolution. This technology uses laser to generate local high temperature on the surface of the substrate, thereby inducing the reduction reaction of copper ions and depositing copper metal on the surface of the substrate. Compared with traditional electroplating and chemical copper plating processes, laser-induced copper deposition technology does not require external current, is flexible to operate and has high precision, and can show great potential in the production of complex structures and tiny patterns.

[0003] However, despite the many advantages of laser-induced copper deposition technology, the current solution formulation still has many problems in practical applications: formaldehyde is used as a reducing agent when preparing copper ion solution, and there are two basic chemical reactions in the reaction process, namely, copper ions obtain electrons to become copper elements, and formaldehyde reacts with hydroxide ions to produce hydrogen and water and carboxylic acid ions and donate electrons; in addition to the effective redox reaction of copper ions on the catalytic surface and in addition to being reduced to metallic copper by formaldehyde, there are many side reactions. This non-side reaction will reduce the cuprous oxide particles, and the resulting cuprous oxide, copper and extremely fine powder will be suspended in the plating solution, which is difficult to remove by filtration and easily causes the plating solution to decompose.

[0004] If cuprous oxide is co-deposited with copper, the copper deposited layer on the surface of the plated part will be loose and rough, which will result in poor bonding between the copper deposited layer, that is, the copper plating layer, and the substrate of the plated part. In addition, some chemical components in the solution are highly corrosive or toxic, posing a potential threat to the health of operators and environmental safety. The waste liquid treatment is complicated and costly, increasing the environmental burden and production cost of the process. Summary of the invention

[0005] One of the purposes of the present invention is to avoid the shortcomings of the prior art and provide a method for preparing a solution formula for laser induced liquid deposition copper plating. The solution formula for laser induced liquid deposition copper plating obtained by the preparation method has the advantages of environmental protection, stable and uniform deposition process, and the obtained copper plating has the advantages of long service life and high quality.

[0006] A second object of the present invention is to provide a solution formula for laser induced liquid deposition copper plating.

[0007] A third object of the present invention is to provide a copper plating method using laser induced liquid deposition.

[0008] To achieve one of the above purposes, the present invention provides the following technical solutions:

[0009] Provided is a method for preparing a solution formula for laser-induced liquid deposition copper plating.

[0010] The following raw material components are used: copper salt, chelating agent, reducing agent, stabilizer, hydroxyl-containing polymer compound, alkaline agent, nano copper powder;

[0011] The preparation method comprises the following steps:

[0012] S1. Dissolving the copper salt and the chelating agent separately in deionized water to obtain a copper salt solution and a chelating agent solution, and mixing the copper salt solution and the chelating agent solution to obtain a first mixed solution in a transparent blue color;

[0013] S2, adding a reducing agent and a stabilizing agent to the first mixed solution in sequence, mixing them evenly, to obtain a second mixed solution;

[0014] S3, adding an alkaline agent to the second mixed solution, adjusting the pH of the second mixed solution to alkaline, and obtaining a third mixed solution as a copper ion solution system;

[0015] S4, adding a hydroxyl-containing polymer compound to the third mixed solution, mixing evenly, then adding nano copper powder, and mixing evenly again to obtain a solution formula for laser induced liquid deposition copper plating.

[0016] In some embodiments, the weight ratio of copper salt, chelating agent, reducing agent, stabilizer, hydroxyl-containing polymer compound, and nano copper powder is 1.2-1.5: 1.5-2: 1.5-2.2: 0.3-0.9: 0.3-0.8.

[0017] The hydroxyl-containing polymer compound is polyethylene glycol, and the dosage of the hydroxyl-containing polymer compound is 15 g / L to 30 g / L. In S3, the pH is 11 to 13.

[0018] In some embodiments, the copper salt is one or a combination of two or more of copper sulfate pentahydrate, copper chlorate, and copper nitrate.

[0019] In some embodiments, the chelating agent is ethylenediaminetetraacetic acid powder, and when dissolving the ethylenediaminetetraacetic acid powder, sodium hydroxide is added during stirring to dissolve the ethylenediaminetetraacetic acid powder into a transparent solution.

[0020] In some embodiments, the reducing agent is sodium glutamate, glucose, baking soda, or a combination of two or more thereof.

[0021] In some embodiments, the stabilizer is 2-2-bipyridine.

[0022] In some embodiments, the hydroxyl-containing polymer compound is one type or a combination of two or more types.

[0023] In some embodiments, the alkaline agent is sodium hydroxide or potassium hydroxide.

[0024] The beneficial effects of the method for preparing a solution formula of laser-induced liquid phase deposition copper plating of the present invention are as follows:

[0025] The preparation method of the solution of the laser induced liquid phase deposition copper plating of the present invention adds a hydroxyl-containing polymer compound so that the solution formula can form a protective film on the molded copper plating surface, effectively inhibit the oxidation reaction of the copper plating, delay the oxidation process of copper, and improve the quality, stability and service life of the copper plating layer. In addition, nano copper powder is also mixed in, which can promote the uniform deposition of the entire solution formula, help to form a dense and uniform copper plating layer, reduce the generation of holes and cracks, ensure the consistency of the board surface, and improve the quality of the coating. The chelating agent used in the present invention replaces the traditional ammonia water, which is more environmentally friendly, has less impact on operators and the environment, and is more stable in the solution, is not easily affected by external conditions and fails, and helps to maintain the stability and consistency of the solution. The solution formula of the present invention can bring new breakthroughs to the laser induced copper deposition technology and promote the further development and application of this technology in the field of electronic manufacturing.

[0026] To achieve the second objective above, the present invention provides the following technical solutions:

[0027] A solution formula for laser-induced liquid phase deposition copper plating is provided, which is prepared by the preparation method of the solution formula for laser-induced liquid phase deposition copper plating.

[0028] To achieve the third objective above, the present invention provides the following technical solutions:

[0029] A method for copper plating by laser induced liquid deposition is provided. The above-mentioned solution formula of laser induced liquid deposition copper plating is spread on the surface of a substrate, and the laser movement route is controlled to act on the solution formula on the surface of the substrate according to a preset copper plating route to obtain a copper-plated circuit. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 The present invention is a flowchart of a method for preparing a solution for laser-induced liquid deposition copper plating according to a specific embodiment of the present invention. DETAILED DESCRIPTION

[0031] The preferred embodiments of the present invention will be described in more detail below with reference to the accompanying drawings. Although the preferred embodiments of the present invention are shown in the accompanying drawings, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments described herein. On the contrary, these embodiments are provided to make the present invention more thorough and complete, and to fully convey the scope of the present invention to those skilled in the art.

[0032] Example

[0033] The preparation method of the solution formula of the laser induced liquid deposition copper plating disclosed in this embodiment is as follows: Figure 1 As shown, the following raw material components are used in the following formula amounts: copper salt, chelating agent, reducing agent, stabilizer, hydroxyl-containing polymer compound, alkaline agent, nano copper powder;

[0034] The preparation method comprises the following steps:

[0035] S1. Dissolving the copper salt and the chelating agent separately in deionized water to obtain a copper salt solution and a chelating agent solution, and mixing the copper salt solution and the chelating agent solution to obtain a first mixed solution in a transparent blue color;

[0036] Specifically, the copper salt solution is slowly injected into the chelating agent solvent along an auxiliary tool such as a glass rod, and stirred evenly.

[0037] S2, adding a reducing agent and a stabilizing agent to the first mixed solution in sequence, mixing them evenly, to obtain a second mixed solution;

[0038] S3, adding an alkaline agent to the second mixed solution, adjusting the pH of the second mixed solution to alkaline, and obtaining a third mixed solution of a copper ion solution system;

[0039] Specifically, the desired copper ion solution system can be obtained by adjusting the solution to alkalinity with an alkaline reagent.

[0040] S4, adding a hydroxyl-containing polymer compound to the third mixed solution, mixing evenly, then adding nano copper powder, and mixing evenly again to obtain a solution formula for laser induced liquid deposition copper plating.

[0041] Specifically, the hydroxyl-containing polymer compound can form a protective film on the surface of the final copper plating layer, inhibiting the oxidation reaction of copper and delaying the oxidation process of copper. Adding nano copper powder to the mixture can promote the deposition rate of copper, help form a dense copper plating layer, reduce the generation of holes and cracks, and improve the quality of the plating layer.

[0042] In this embodiment, copper salt, chelating agent, reducing agent, stabilizer, hydroxyl-containing polymer compound, nano copper powder = 1.2-1.5: 1.5-2: 1.5-2.2: 0.3-0.9: 0.3-0.8,

[0043] The weight ratio of the above raw material components can be adjusted according to actual conditions, wherein:

[0044] The copper salt can be 0.01 to 0.5 g / ml;

[0045] The chelating agent can be 0.02 to 0.4 g / ml;

[0046] The reducing agent can be 0.1 to 0.3 g / ml;

[0047] The stabilizer can be 0.01-0.2 g / ml;

[0048] The hydroxyl-containing polymer compound is polyethylene glycol, and the dosage of the hydroxyl-containing polymer compound is 15 g / L to 30 g / L. In S3, the pH is 11 to 13.

[0049] In this embodiment, the copper salt is one or a combination of two or more of copper sulfate pentahydrate, copper chlorate, and copper nitrate;

[0050] In this embodiment, the chelating agent is ethylenediaminetetraacetic acid powder. When dissolving the ethylenediaminetetraacetic acid powder, sodium hydroxide is added during stirring to dissolve the ethylenediaminetetraacetic acid powder into a transparent solution.

[0051] In this embodiment, the reducing agent is sodium glutamate, glucose, baking soda, or a combination of two or more thereof;

[0052] The use of the above-mentioned reducing agent is environmentally friendly, conforms to green production and does not cause harm to the health of operators.

[0053] It is easy to obtain in the market and the price is relatively low, which can reduce the production cost. At the same time, sodium glutamate and glucose are relatively stable in the solution and are not easily affected by external conditions and become ineffective, which helps to maintain the stability and consistency of the copper precipitation solution.

[0054] In this embodiment, the stabilizer is 2-2 bipyridine;

[0055] In this embodiment, the hydroxyl-containing polymer compound is one or a combination of two or more;

[0056] In this embodiment, the alkaline reagent is sodium hydroxide or potassium hydroxide.

[0057] Experimental example:

[0058] In order to illustrate the effect of the solution formulation of the present invention, the following experimental examples are carried out:

[0059] The method of the present invention is now used to prepare a copper sulfate solution with a concentration of 25g / L and a volume of 50ml for laser-induced copper deposition; a laser machine tool with an ultraviolet nanosecond laser wavelength of 1064λ / nm, a pulse width of 40ns, and a frequency of 300kHz is used for laser induction, and the substrate is a high borosilicate glass with a silicon content of >80%, a size of 40×40×1mm, and a thermal conductivity of 1.2W / m·K. Specifically, the concentrations of the raw material components are shown in Table 1:

[0060] Table 1

[0061]

[0062] Use a balance to weigh 1.25g of copper sulfate pentahydrate, 1.75g ​​of EDTA, 1.3g of sodium glutamate, and an appropriate amount of sodium hydroxide;

[0063] Dissolve copper sulfate pentahydrate, sodium glutamate, and 25 g of sodium hydroxide in deionized water respectively, and stir with a glass plate to prepare a 25 g / L copper sulfate solution, a 26 g / L sodium glutamate solution, and a sodium hydroxide solution with a pH of 12.2 to 12.8;

[0064] Put ethylenediaminetetraacetic acid powder into a beaker, add deionized water to dissolve, place the obtained suspension on a magnetic stirrer for stirring, then add a certain amount of sodium hydroxide solution and stir until transparent;

[0065] Add EDTA solution to the copper sulfate solution and stir until a transparent blue mixed solution appears;

[0066] adding the sodium glutamate solution into the mixed solution;

[0067] Add 0.4g-0.83g of stabilizer 2-2-bipyridine and stir evenly;

[0068] Pour the prepared sodium hydroxide solution into the above mixed solution until the pH of the solution is 12.2-12.8, then add 20 g / L polyethylene glycol;

[0069] Finally, 0.5 g of nano copper powder was added into the mixed solution.

[0070] Experimental results:

[0071] The prepared solution is spread on the glass surface, and the glass plate covered with the copper ion solution is acted on by laser. The line width of the copper wire produced is 5% to 10% narrower than that of the copper wire produced by the prior art, the uniformity of the copper wire is increased by 20% to 40%, the adhesion is increased by 30% to 60% through the tensile test, the conductivity is increased by 10%-30%, and the holes and cracks are reduced by 30% to 50%. It can be seen that the present invention can produce better.

[0072] Unless otherwise specifically stated, the relative arrangement, numerical expressions and numerical values ​​of the parts and steps set forth in these embodiments do not limit the scope of the present application. At the same time, it should be understood that, for ease of description, the sizes of the various parts shown in the accompanying drawings are not drawn according to the actual proportional relationship. The technology, method and equipment known to those of ordinary skill in the relevant field may not be discussed in detail, but in appropriate cases, the technology, method and equipment should be considered as a part of the authorization specification. In all examples shown and discussed here, any specific value should be interpreted as being merely exemplary, rather than as a limitation. Therefore, other examples of exemplary embodiments may have different values. It should be noted that similar reference numerals and letters represent similar items in the following drawings, so that once a certain item is defined in an accompanying drawing, it does not need to be further discussed in subsequent drawings.

[0073] In the description of the present application, it should be understood that the directions or positional relationships indicated by directional words such as "front, back, up, down, left, right", "lateral, vertical, perpendicular, horizontal" and "top, bottom" are usually based on the directions or positional relationships shown in the drawings, and are only for the convenience of describing the present application and simplifying the description. Unless otherwise specified, these directional words do not indicate or imply that the device or element referred to must have a specific direction or be constructed and operated in a specific direction, and therefore cannot be understood as limiting the scope of protection of the present application; the directional words "inside and outside" refer to the inside and outside relative to the contours of each component itself.

[0074] For ease of description, spatially relative terms such as "above", "above", "on the upper surface of", "above", etc. may be used here to describe the spatial positional relationship between a device or feature and other devices or features as shown in the figure. It should be understood that spatially relative terms are intended to include different orientations of the device in use or operation in addition to the orientation described in the figure. For example, if the device in the accompanying drawings is inverted, the device described as "above other devices or structures" or "above other devices or structures" will be positioned as "below other devices or structures" or "below other devices or structures". Thus, the exemplary term "above" can include both "above" and "below". The device can also be positioned in other different ways (rotated 90 degrees or in other orientations), and the spatially relative descriptions used here are interpreted accordingly.

[0075] In addition, it should be noted that the use of terms such as "first" and "second" to limit components is only for the convenience of distinguishing the corresponding components. Unless otherwise stated, the above terms have no special meaning and therefore cannot be understood as limiting the scope of protection of this application.

[0076] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a solution formula for laser-induced liquid deposition copper plating, It is characterized in that The following raw material components are used: copper salt, chelating agent, reducing agent, stabilizer, hydroxyl-containing polymer compound, alkaline agent, and nano copper powder; The preparation method comprises the following steps: S1. Dissolving the copper salt and the chelating agent separately in deionized water to obtain a copper salt solution and a chelating agent solution, and mixing the copper salt solution and the chelating agent solution to obtain a first mixed solution in a transparent blue color; S2, adding a reducing agent and a stabilizing agent to the first mixed solution in sequence, mixing them evenly, to obtain a second mixed solution; S3, adding an alkaline agent to the second mixed solution to adjust the pH of the second mixed solution to alkaline, thereby obtaining a third mixed solution as a copper ion solution system; S4, adding a hydroxyl-containing polymer compound to the third mixed solution, mixing evenly, then adding nano copper powder, and mixing evenly again to obtain a solution formula for laser induced liquid deposition copper plating.

2. The method for preparing the solution formula of laser induced liquid deposition copper plating according to claim 1, It is characterized in that The weight ratio of copper salt, chelating agent, reducing agent, stabilizer, hydroxyl-containing polymer compound and nano copper powder is 1.2-1.5:1.5-2:1.5-2.2:0.3-0.9:0.3-0.

8. The hydroxyl-containing polymer compound is polyethylene glycol, and the amount of the hydroxyl-containing polymer compound is 15 g / L to 30 g / L. In S3, the pH is 11-13.

3. The method for preparing the solution formula of laser induced liquid deposition copper plating according to claim 1, It is characterized in that The copper salt is one or a combination of two or more of copper sulfate pentahydrate, copper chlorate and copper nitrate.

4. The method for preparing the solution formula of laser induced liquid deposition copper plating according to claim 1, It is characterized in that The chelating agent is ethylenediaminetetraacetic acid powder. When dissolving the ethylenediaminetetraacetic acid powder, sodium hydroxide is added during stirring to dissolve the ethylenediaminetetraacetic acid powder into a transparent solution.

5. The method for preparing the solution formula of laser induced liquid deposition copper plating according to claim 1, It is characterized in that The reducing agent is sodium glutamate, glucose, baking soda, or a combination of two or more thereof.

6. The method for preparing the solution formula of laser induced liquid deposition copper plating according to claim 1, It is characterized in that The stabilizer is 2-2-bipyridine.

7. The method for preparing the solution formula of laser induced liquid deposition copper plating according to claim 1, It is characterized in that The hydroxyl-containing polymer compound is one or a combination of two or more.

8. The method for preparing the solution formula of laser induced liquid deposition copper plating according to claim 1, It is characterized in that The alkaline agent is sodium hydroxide or potassium hydroxide.

9. A solution formula for laser-induced liquid deposition copper plating, It is characterized in that The copper plating solution is prepared by the method for preparing the solution formula of laser induced liquid deposition copper plating according to any one of claims 1 to 8.

10. A copper plating method using laser induced liquid deposition, It is characterized in that The laser-induced liquid deposition copper plating solution formula according to any one of claims 1 to 8 is spread on the surface of the substrate, and the laser movement route is controlled to act on the solution formula on the surface of the substrate according to a preset copper plating route to obtain a copper-plated circuit.

Citation Information

Patent Citations

  • Multi-layer circuit board preparation method

    CN117641772A

  • Method for preparing multilayer circuit board by laser

    CN117641773A