Foam metal catalyst with modified catalytic sites, preparation method of foam metal catalyst and application of foam metal catalyst in electrolyzed water and seawater
Through the reaction of foam metal with hydrogen peroxide and nitrogen-containing compounds under hydrothermal conditions, the catalytic site is optimized to form an efficient oxygen reduction electrocatalyst, which solves the problems of easy deactivation of precious metal catalysts and corrosion of chloride ions in seawater, and achieves the High-efficiency hydrogen production in electrolytic water and seawater reduces costs and improves stability.
Patent Information
- Application Number
- CN202411220837.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-11-08
AI Technical Summary
Existing precious metal catalysts such as ruthenium oxide (RuO2) and iridium oxide (IrO2) are prone to deactivate and costly during the process of electrolyzing hydrogen production, and high concentration of chloride ion corrosion catalysts in seawater, resulting in a decrease in the production efficiency and stability of electrolyzed hydrogen.
By reacting foam metal with hydrogen peroxide and nitrogen-containing compounds under hydrothermal conditions, the valence state of the catalytic site is optimized to form an efficient oxygen reduction (OER) electrocatalyst, replacing precious metal catalysts, and generating negative ions through nitrogen-containing atoms. The partition layer prevents chloride ions from corrosion.
It realizes efficient and stable hydrogen production in electrolytic water and seawater, reduces the production cost of catalysts, improves the corrosion resistance and electrocatalytic activity of the catalysts, and provides a feasible solution to solve energy crises and environmental pollution.
Smart Images

Figure CN118910640A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of catalysis, and in particular relates to a catalytic site-modified foam metal catalyst, a preparation method thereof, and application in electrolyzing water and seawater. Background Art
[0002] Developing clean and renewable energy is one of the important ways to achieve sustainable development. Hydrogen is considered to be the most ideal energy carrier due to its high energy density and non-polluting products. Water electrolysis is considered to be the most promising way to produce hydrogen because of its simplicity and high efficiency.
[0003] The oxygen evolution reaction (OER) is the controlling step in hydrogen production by water electrolysis. The formation of oxygen active species in the reaction process requires overcoming a huge energy barrier, and the catalyst is easily deactivated, which seriously restricts the efficiency of water electrolysis.
[0004] At present, noble metal catalysts such as ruthenium oxide (RuO2) and iridium oxide (IrO2) are recognized as efficient OER electrocatalysts. However, these raw materials are not only expensive but also scarce, which greatly limits the commercial application of such catalysts. Therefore, it is of great significance to design and construct efficient and stable OER electrocatalysts based on elements with abundant reserves on the earth.
[0005] At the same time, compared with scarce freshwater resources, seawater is considered to be an ideal substitute for its abundant resources and can achieve large-scale production of hydrogen. Unfortunately, the high concentration of chloride ions (about 0.5M) in seawater will corrode the active sites of the anode catalyst of water electrolysis during the OER reaction, causing the activity and stability of the catalyst to drop sharply. Constructing OER sites that are resistant to chloride ion corrosion is still a huge challenge.
[0006] The patent with publication number CN 115717252 A published on February 28, 2023 discloses a preparation method and application of a bifunctional catalyst for seawater electrolysis. First, the Cu2SeS active component is prepared on a nickel foam substrate by a solvothermal method, and then the CoZnLDH grid-like structure material formed by the interlacing of nanosheets is loaded on the prepared Cu2SeS / nickel foam by a hydrothermal method to obtain a CoZnLDH-Cu2SeS / nickel foam composite material, and finally the CoZnLDH-Cu2SeS / nickel foam is thermally phosphated to finally obtain a P-CoZnO-Cu2SeS / nickel foam bifunctional catalyst with a grid-like structure. The catalyst has both high catalytic activity for seawater electrolysis and strong resistance to corrosion by chloride ions in seawater. However, its preparation method is complicated and requires multiple steps and raw materials. Summary of the invention
[0007] The purpose of the present invention is to provide a catalytic site modified foam metal catalyst and a preparation method thereof, using foam metal as a raw material, modified with hydrogen peroxide and a nitrogen-containing compound, optimizing the valence state of the catalytic site and improving its microenvironment through a hydrothermal reaction, thereby constructing an efficient and corrosion-resistant OER electrocatalyst; the preparation method of the present invention is simple and the preparation cost is low, and it replaces traditional precious metal catalysts.
[0008] Another object of the present invention is to provide a catalytic site-modified foam metal catalyst for use in the electrolysis of water and seawater, which has excellent OER electrocatalytic activity. Its application in the field of electrolysis of water and seawater can provide a practical idea for solving the increasingly serious energy crisis and environmental pollution problems.
[0009] The specific technical solutions of the present invention are as follows:
[0010] A method for preparing a catalytic site-modified foamed metal catalyst, specifically comprising:
[0011] The foamed metal and the nitrogen-containing compound are mixed in a hydrogen peroxide solution and subjected to a hydrothermal reaction to obtain a foamed metal catalyst with modified catalytic sites.
[0012] The ratio of the foam metal area to the volume of the hydrogen peroxide solution is: 1-6 cm 2 :5-20mL;
[0013] The foam metal is cleaned before use, and the cleaning process is: the foam metal is ultrasonically treated in acetone, ethanol, 1-6 mol / L HCl solution and pure water for 5-15 minutes in sequence, and then dried for later use;
[0014] The foam metal includes any one of foam nickel, foam iron nickel, foam nickel aluminum or foam nickel molybdenum;
[0015] The concentration of the nitrogen-containing compound in the hydrogen peroxide solution is 10-200 mg / ml;
[0016] The nitrogen-containing compound is any one of urea, ammonia water or hydrazine hydrate;
[0017] The solvent of the hydrogen peroxide solution is a mixed solvent of water and alcohol in any proportion; the alcohol is selected from any one or more of methanol, ethanol or ethylene glycol; the water is pure water; the solvent of the hydrogen peroxide solution is preferably pure water;
[0018] The concentration of the hydrogen peroxide solution ranges from 1 wt% to 20 wt%.
[0019] The hydrothermal reaction refers to: reacting at 80-160°C for 4-48 hours;
[0020] After the hydrothermal reaction is completed, the metal foam is washed with water and alcohol in sequence, and vacuum dried at 30-60° C. to a constant weight, thereby obtaining a metal foam catalyst with modified catalytic sites.
[0021] The present invention uses foamed metal as a matrix, mixes it with nitrogen-containing compounds in a hydrogen peroxide solution, and then undergoes a hydrothermal reaction to prepare a modified foamed metal catalyst, which exhibits excellent OER activity. Nitrogen-containing compounds and hydrogen peroxide are cheap and readily available. Under hydrothermal conditions, hydrogen peroxide and foamed nickel undergo an oxidation-reduction reaction to generate Ni on the surface of the foamed nickel. 2+ , nitrogen-containing molecules react with Ni under hydrothermal conditions 2+ The species are coordinated, the electronic structure of the active site is optimized, which is beneficial to the adsorption and desorption of oxygen active species, and some nitrogen-containing species can be converted into negatively charged anions in situ during the OER process, which can effectively hinder the poisoning effect of chloride ions. The present invention uses transition metals as raw materials, and uses hydrogen peroxide and nitrogen-containing compounds for modification, replacing traditional precious metal catalysts, and provides a cheap, easily available and highly active electrocatalyst for water electrolysis OER.
[0022] The present invention provides a foamed metal catalyst with modified catalytic sites, which is prepared by the above method. The method obtains nitrogen-modified 10-80 nm metal oxide nanoparticles tightly loaded on the surface of the foamed nickel.
[0023] The present invention provides a foamed metal catalyst with modified catalytic sites for use in electrolysis of water and seawater. In a 1.0M KOH solution, the modified foamed nickel material reaches 300 mA·cm -2 The overpotential is between 260-400 mV vs. RHE; in 1.0 M KOH + seawater medium, it reaches 300 mA cm -2 The overpotential of the modified nickel foam is between 270-430mV vs. RHE. In addition, due to the combined effect of urea and hydrogen peroxide, the modified nickel foam has a higher overpotential than the single urea-modified and hydrogen peroxide-modified nickel foam at 300mA·cm -2 The overpotential decreased by 10-200 mV in 1.0 M KOH and 1.0 M KOH + seawater, respectively.
[0024] Compared with the prior art, the present invention is prepared under hydrothermal conditions, hydrogen peroxide easily undergoes oxidation reaction with foamed metals (Ni, Fe, Al, Mo), and nitrogen-containing compounds undergo coordination reaction therewith to improve the valence state of metal sites, which is beneficial to the adsorption and desorption of oxygen active species, and the negative electron barrier layer generated in situ by nitrogen atoms can effectively hinder the poisoning effect of chloride ions on active sites due to electrostatic repulsion. The preparation method is simple, the raw materials are cheap and easily available, and the prepared catalyst has excellent OER electrocatalytic activity. Applying it in the field of water electrolysis and seawater electrolysis can provide a practical idea for solving the increasingly serious energy crisis and environmental pollution problems. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 The X-ray powder diffraction XRD pattern of the modified nickel foam obtained in Example 1;
[0026] Figure 2 This is a scanning electron microscope photograph of the modified nickel foam obtained in Example 1;
[0027] Figure 3 The XPS spectra of Ni 2p of the modified nickel foam and the original nickel foam obtained in Example 1;
[0028] Figure 4 This is the XPS spectrum of N1s of the modified nickel foam obtained in Example 1;
[0029] Figure 5 The LSV curve of the oxygen evolution reaction of the modified nickel foam obtained in Example 1 in 1.0M KOH;
[0030] Figure 6 This is the LSV curve of the oxygen evolution reaction of the modified nickel foam obtained in Example 1 in 1.0M KOH+seawater.
[0031] Figure 7 The LSV curve of the oxygen evolution reaction of the nickel foam modified with hydrogen peroxide alone in 1.0M KOH obtained in Comparative Example 1;
[0032] Figure 8 This is the LSV curve of the oxygen evolution reaction of the single hydrogen peroxide-modified nickel foam obtained in Comparative Example 1 in 1.0M KOH+seawater;
[0033] Fig. 9 The LS V curve of the oxygen evolution reaction of the single urea-modified nickel foam obtained in Comparative Example 2 in 1.0 M KOH;
[0034] Fig.10 This is the LSV curve of the oxygen evolution reaction of the single urea-modified nickel foam obtained in Comparative Example 2 in 1.0M KOH+seawater;
[0035] Fig.11The LSV curve of the oxygen evolution reaction of the unmodified nickel foam obtained in Comparative Example 3 in 1.0M KOH;
[0036] Fig.12 This is the LSV curve of the oxygen evolution reaction of the modified nickel foam obtained in Example 2 in 1.0M KOH;
[0037] Fig.13 The LSV curve of the oxygen evolution reaction of the modified nickel-iron foam obtained in Example 3 in 1.0M KOH;
[0038] Fig.14 This is the LSV curve of the oxygen evolution reaction of the unmodified and cleaned nickel-iron foam obtained in Example 3 in 1.0 M KOH. DETAILED DESCRIPTION
[0039] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0040] Unless otherwise specified, the test materials and reagents used in the following examples can be obtained from commercial sources.
[0041] If no specific techniques or conditions are specified in the examples, they can be carried out according to the techniques or conditions described in the literature in the art or according to the product instructions.
[0042] The foam metals used below were cleaned before use. The cleaning process was as follows: the foam metals were ultrasonically treated in acetone, ethanol, 2 mol / L HCl solution and pure water for 5-15 min in turn, and then dried for later use.
[0043] Example 1
[0044] A method for preparing a catalytic site-modified foamed metal catalyst comprises the following steps:
[0045] A. Dispersion: Add the cleaned 0.5 cm × 2 cm nickel foam and 6 mmol urea to 15 mL 5 wt% hydrogen peroxide solution and stir for 10 min. Then transfer all to a hydrothermal reactor and react at 120 °C for 16 h.
[0046] B. Drying: The system after the reaction is cooled and separated, and the precipitate is first washed with water and then with alcohol, and then vacuum dried at 40° C. to a constant weight, thereby obtaining a modified metal foam oxygen evolution reaction catalyst marked as Ni-UH.
[0047] Figure 1 The X-ray powder diffraction XRD pattern of the modified nickel foam obtained in Example 1 mainly shows the diffraction peak of Ni;
[0048] Figure 2 This is a scanning electron microscope photo of the modified nickel foam obtained in Example 1; from the photo, it can be seen that nanoparticles of about 50 nm are densely loaded on the surface of the nickel foam;
[0049] Figure 3 XPS spectra of Ni 2p of the modified nickel foam (Ni-UH) and the original nickel foam (Ni) obtained in Example 1; Figure 4 The XPS spectrum of N1s of the modified nickel foam obtained in Example 1; XPS test proves that the electronic structure of Ni-UH is changed relative to the original nickel foam (Ni), and the valence state of the surface of the modified nickel foam is mainly +2 relative to the cleaned nickel foam, which proves the generation of NiO species and the successful coupling of nitrogen-containing species with NiO substances ( Figure 3 and Figure 4 ), which is conducive to the adsorption and desorption of oxygen active species on the surface of nickel foam.
[0050] The application of a catalytic site-modified foam metal catalyst in the electrolysis of water and seawater. The specific electrocatalytic performance test is as follows:
[0051] The nickel foam with modified catalytic sites obtained in Example 1 was used as a catalyst for the electrocatalytic reaction of OER:
[0052] The prepared catalytic site-modified nickel foam was inserted into 1.0M KOH with an area of 0.5 cm×1.0 cm, and the electrocatalytic process of oxygen evolution reaction was recorded by an electrochemical workstation in the potential window of 1.20-1.61 V vs. RHE. It can be seen that when the current density reaches 300 mA cm -2 When the overpotential is only 350mV vs.RHE, see Figure 5 ; and at 300mA·cm -2 After working continuously for 24 hours, the current density decay is less than 5%.
[0053] The prepared modified nickel foam was immersed in 1.0M KOH + seawater 0.5cm×1.0cm, and the electrocatalytic process of oxygen evolution reaction was recorded by an electrochemical workstation in the potential window of 1.20-1.62V vs. RHE. It can be seen that when the current density reaches 300mA·cm -2 When the overpotential is only 360mV vs.RHE, see Figure 6 , and at 300mA·cm -2 After working continuously for 24 hours, the current density decay is less than 5%.
[0054] Comparative Example 1
[0055] A method for preparing a single hydrogen peroxide-modified nickel foam catalyst comprises the following steps:
[0056] A. Dispersion: Add the cleaned 0.5 cm × 2 cm nickel foam to 15 mL of 5 wt% hydrogen peroxide solution and stir for 10 min, then transfer all to a hydrothermal reactor and react at 120 °C for 16 h;
[0057] B. Drying: The system after the reaction is cooled and separated, and the precipitate is first washed with water and then with alcohol, and then vacuum dried at 40°C to constant weight to obtain a modified metal foam oxygen evolution reaction catalyst, which is marked as Ni-H.
[0058] The application of a single hydrogen peroxide modified nickel foam catalyst in the electrolysis of water and seawater. The specific electrocatalytic performance test is as follows:
[0059] The single hydrogen peroxide-modified nickel foam obtained in Comparative Example 1 was used as a catalyst for the electrocatalytic reaction of OER:
[0060] The prepared nickel foam was inserted into 1.0M KOH with an area of 0.5cm×1.0cm, and the electrocatalytic process of oxygen evolution reaction was recorded by an electrochemical workstation in the potential window of 1.2-1.80V vs.RHE. It can be seen that when the current density reaches 300mA·cm -2 When the overpotential is 483mV vs.RH E, see Figure 7 ;
[0061] The prepared modified nickel foam was immersed in 1.0M KOH + seawater 0.5cm×1.0cm, and the electrocatalytic process of oxygen evolution reaction was recorded by an electrochemical workstation in the potential window of 1.2-1.90V vs. RHE. It can be seen that when the current density reaches 300mA·cm -2 When the overpotential is 625mV vs.RHE, see Figure 8 .
[0062] Comparative Example 2
[0063] A method for preparing a single urea-modified nickel foam catalyst comprises the following steps:
[0064] A. Dispersion: Add the cleaned 0.5 cm × 2 cm nickel foam and 6 mmol urea into 15 mL pure water solution and stir for 10 min, then transfer all to a hydrothermal reactor and react at 120 ° C for 16 h;
[0065] B. Drying: The system after the reaction is cooled and separated, and the precipitate is first washed with water and then with alcohol, and then vacuum dried at 40°C to constant weight to obtain a single urea-modified metal foam oxygen evolution reaction catalyst, which is marked as Ni-U.
[0066] The application of a single urea-modified nickel foam catalyst in the electrolysis of water and seawater. The specific electrocatalytic performance test is as follows:
[0067] The single urea-modified nickel foam obtained in Comparative Example 2 was used as a catalyst for the electrocatalytic reaction of OER:
[0068] The prepared nickel foam was inserted into 1.0M KOH with an area of 0.5cm×1.0cm, and the electrocatalytic process of oxygen evolution reaction was recorded by an electrochemical workstation in the potential window of 1.2-1.80V vs.RHE. It can be seen that when the current density reaches 300mA·cm -2 When the overpotential is only 524mV vs.RHE, see Fig. 9 ;
[0069] The prepared modified nickel foam was immersed in 1.0M KOH + seawater 0.5cm×1.0cm, and the electrocatalytic process of oxygen evolution reaction was recorded by an electrochemical workstation in the potential window of 1.2-2.0V vs. RHE. It can be seen that when the current density reaches 300mA·cm -2 When the overpotential is only 726mV vs.RHE, see Fig.10 .
[0070] Comparative Example 3
[0071] Electrochemical test of oxygen evolution reaction of nickel foam without modification with hydrogen peroxide or urea and only for cleaning:
[0072] The unmodified nickel foam that was only cleaned was inserted into 1.0M KOH with an area of 0.5cm×1.0cm, and the electrocatalytic process of oxygen evolution reaction was recorded by an electrochemical workstation in the potential window of 1.2~1.90V vs.RHE. It can be seen that when the current density reaches 300mA·cm -2 When the overpotential is as high as 550mV vs.RHE, see Fig.11 , the activity is weak, which proves that hydrogen peroxide and urea have a great effect on the modification of foam catalytic sites.
[0073] Example 2
[0074] A method for preparing a catalytic site-modified foamed metal catalyst comprises the following steps:
[0075] A. Dispersion: Add the cleaned 0.5 cm×2 cm nickel foam and 3 mmol urea to 10 mL 5 wt% hydrogen peroxide solution and stir for 10 min. Then transfer all to a hydrothermal reactor and react at 120°C for 16 h.
[0076] B. Drying: The system after the reaction is cooled and separated, and the precipitate is first washed with water and then with alcohol, and then vacuum dried at 40° C. to a constant weight, thereby obtaining a modified metal foam oxygen evolution reaction catalyst marked as Ni-UH-2.
[0077] The application of a catalytic site-modified foam metal catalyst in the electrolysis of water and seawater. The specific electrocatalytic performance test is as follows:
[0078] The nickel foam with modified catalytic sites obtained in Example 2 was used as a catalyst for the electrocatalytic reaction of OER:
[0079] The prepared catalytic site-modified nickel foam was inserted into 1.0 M KOH with an area of 0.5 cm × 1.0 cm, and the electrocatalytic process of oxygen evolution reaction was recorded by an electrochemical workstation in the potential window of 1.20 to 1.66 V vs. RHE. It can be seen that when the current density reaches 300 mA cm -2 When the overpotential is only 386mV vs.RHE, see Fig.12 ;
[0080] The prepared modified nickel foam was immersed in 1.0M KOH + seawater 0.5cm×1.0cm, and the electrocatalytic process of oxygen evolution reaction was recorded by an electrochemical workstation in the potential window of 1.20-1.75V vs. RHE. It can be seen that when the current density reaches 300mA·cm -2 Its overpotential is only 405mVvs.RHE.
[0081] Example 3
[0082] A method for preparing a catalytic site-modified foamed metal catalyst comprises the following steps:
[0083] A. Dispersion: Add the cleaned 1 cm×2.5 cm foamed iron-nickel and 10 mmol urea to 20 mL 5 wt% hydrogen peroxide solution and stir for 10 min, then transfer all to a hydrothermal reactor and react at 120°C for 16 h;
[0084] B. Drying: The system after the reaction is cooled and separated, and the precipitate is first washed with water and then with alcohol, and then vacuum dried at 30° C. to constant weight to obtain a modified metal foam oxygen evolution reaction catalyst, which is marked as NiFe-UH.
[0085] The application of a catalytic site-modified foam metal catalyst in the electrolysis of water and seawater. The specific electrocatalytic performance test is as follows:
[0086] The foamed metal catalyst with modified catalytic sites obtained in Example 3 was used as a catalyst for the electrocatalytic reaction of OER:
[0087] The improved nickel-iron foam prepared in Example 3 was inserted into 1.0 M KOH with an area of 1.0 cm×1.0 cm, and the electrocatalytic process of oxygen evolution reaction was recorded by an electrochemical workstation in a potential window of 1.2 to 1.57 V vs. RHE. It can be seen that when the current density reaches 300 mA cm -2 When the overpotential is only 293mV vs.RHE, see Fig.13 ;
[0088] The prepared modified nickel-iron foam was immersed in 1.0M KOH + seawater (0.5 cm × 1.0 cm), and the electrocatalytic process of oxygen evolution reaction was recorded by an electrochemical workstation in the potential window of 1.2 to 1.65 V vs. RHE. It can be seen that when the current density reaches 300 mA cm -2 Its overpotential is 340mV vs.RHE.
[0089] The cleaned and unmodified nickel foam used in Example 3 was used as a catalyst for the electrocatalytic reaction of oxygen evolution reaction:
[0090] First, the cleaned Fe-Ni foam without modification was immersed in 1.0 M KOH 1.0 cm × 1.0 cm, and the electrocatalytic process of oxygen evolution reaction was recorded by an electrochemical workstation in the potential window of 1.2 to 1.63 vs. RHE. It can be seen that when the current density reaches 300 mA cm -2 Its overpotential is 328mV vs.RHE( Fig.14 );
[0091] The untreated Fe-Ni foam was immersed in 1.0 M KOH + seawater (1.0 cm × 1.0 cm), and the electrocatalytic process of oxygen evolution reaction was recorded by an electrochemical workstation in the potential window of 1.2 to 1.75 V vs. RHE. It can be seen that when the current density reaches 300 mA cm -2 Its overpotential is 396mV vs.RHE.
[0092] In the present invention, hydrogen peroxide can improve the valence state of the active site, the nitrogen-containing compound is easy to coordinate with Ni to improve the electronic structure of the active site, and the negative ion barrier layer formed in the electrochemical process hinders the poisoning effect of chloride ions on the active site. By regulating the amount of hydrogen peroxide and nitrogen-containing compounds, the electronic structure of the active site and the negative ion barrier layer can be regulated, the adsorption energy barrier of the active species can be optimized, the reaction kinetics can be improved, and when the amount of urea and hydrogen peroxide is reduced, the OER activity of the obtained material is reduced; the negative ion barrier layer can effectively hinder the poisoning of the active site by chloride ions due to electrostatic repulsion.
[0093] The description of the above embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the protection scope of the present invention.
Claims
1. A method for preparing a catalytic site-modified foamed metal catalyst, characterized in that: The preparation method is specifically: The foamed metal and the nitrogen-containing compound are mixed in a hydrogen peroxide solution and subjected to a hydrothermal reaction to obtain a foamed metal catalyst with modified catalytic sites.
2. The preparation method according to claim 1, characterized in that: The foam metal includes any one of foam nickel, foam iron nickel, foam nickel aluminum or foam nickel molybdenum.
3. The preparation method according to claim 1, characterized in that: The concentration of the nitrogen-containing compound in the hydrogen peroxide solution is 10-200 mg / ml.
4. The preparation method according to claim 1 or 3, characterized in that: The nitrogen-containing compound is any one of urea, ammonia water or hydrazine hydrate.
5. The preparation method according to claim 1, characterized in that: The solvent of the hydrogen peroxide solution is a mixed solvent of water and alcohol in any proportion.
6. The preparation method according to claim 1 or 5, characterized in that: The concentration of the hydrogen peroxide solution ranges from 1 wt% to 20 wt%.
7. The preparation method according to claim 1, characterized in that: The hydrothermal reaction refers to: reacting at 80-160° C. for 4-48 hours.
8. A foamed metal catalyst with modified catalytic sites prepared by the preparation method according to any one of claims 1 to 7.
9. Use of the catalytic site-modified foam metal catalyst according to claim 8 for electrolysis of water.
10. Use of the catalytic site-modified foam metal catalyst according to claim 8 for electrolysis of seawater.