Copper electrocatalyst for producing ammonia by electrochemically reducing nitrate and preparation method of copper electrocatalyst
By simplifying the preparation process of copper material electrocatalysts, using foam copper substrate and copper film active components to form a three-dimensional porous copper electrocatalyst, solving the problems of complex preparation and low ammonia production rate in the prior art, achieving high efficiency and stability Electrocatalytic performance and low-cost process.
Patent Information
- Application Number
- CN202411238314.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-11-08
AI Technical Summary
The existing copper electrocatalyst preparation process is complex, time-consuming and low ammonia production rate, which cannot meet the needs. The high cost and scarce reserves of precious metal catalysts are limited, which limits large-scale applications.
Using foam copper as the substrate, copper film active components are prepared by pretreatment, electrodeposition and heat treatment to form a three-dimensional porous copper electrocatalyst, simplifying the process flow and reducing raw material costs.
It achieves high-efficiency electrocatalytic rate and stability, reduces raw material costs, simplifies the preparation process, avoids the later modification steps, and significantly improves the Faraday efficiency and stability of ammonia production.
Smart Images

Figure CN118910652A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of catalysts, and in particular to a copper electrocatalyst for electrochemically reducing nitrate to produce ammonia and a preparation method thereof. Background Art
[0002] The electrocatalysts for nitrate reduction to ammonia mainly include non-metallic, non-precious metal, precious metal and other materials. Although the electrocatalytic performance of materials containing precious metals is relatively high, precious metals are expensive and scarce, which limits the mass preparation of materials and the large-scale application of technology. Copper materials have good conductivity and weak hydrogen evolution ability, and can be used to make electrocatalysts for nitrate reduction to ammonia; however, the existing copper material electrocatalysts still have the following defects: First, there are many preparation steps and the process is relatively complicated, resulting in a long time consumption; second, the prepared copper material electrocatalysts need post-processing before they can be used, and the post-processing is to modify the prepared catalyst on the substrate with a conductive adhesive; third, the ammonia production rate of the existing copper material electrocatalysts is low and can no longer meet the demand. Summary of the invention
[0003] The object of the present invention is to provide a copper electrocatalyst for electrochemical reduction of nitrate to produce ammonia and a preparation method thereof, so as to solve the problems raised in the above background technology.
[0004] To achieve the above object, the present invention provides the following technical solution: a copper electrocatalyst for electrochemical reduction of nitrate to produce ammonia, comprising a substrate and an active component, wherein the substrate is foamed copper and the active component is a copper film.
[0005] A method for preparing a copper electrocatalyst for electrochemical reduction of nitrate to produce ammonia, comprising the steps of: first, pretreatment of a substrate; second, electrodeposition to generate an active component; and third, heat treatment to obtain the copper electrocatalyst;
[0006] In the above step 1, the copper foam is pretreated to remove the oxide layer and organic matter on the surface;
[0007] In the above step 2, the copper foam pretreated in step 1 is taken, the copper foam is clamped by a platinum electrode clamp and placed in a single-chamber reaction tank filled with an electroplating solution, the copper foam is used as a counter electrode, the two electrode sheets are kept parallel, copper is electrodeposited, and a copper film is formed on the surface of the copper foam;
[0008] In the above step three, the copper foam with the copper film formed on the surface in step two is placed in a beaker filled with deionized water for cleaning, and then placed in a tubular furnace for heat treatment. After the heat treatment is completed, a three-dimensional porous copper electrocatalyst is obtained.
[0009] Preferably, in step 1, the pretreatment is specifically: immersing the foamed copper in 1M HCl for ultrasonic cleaning for 3 minutes, then immersing it in anhydrous ethanol for ultrasonic cleaning for 3 minutes, and finally immersing it in deionized water for ultrasonic cleaning for 3 minutes.
[0010] Preferably, the area of the copper foam is 0.5 cm×0.5 cm.
[0011] Preferably, in step 2, the composition of the electroplating solution is: 0.015M CuSO4+0.15M K2SO4+0.03MH2SO4.
[0012] Preferably, in step 2, the effective volume of the single-chamber reaction pool is 50 ml.
[0013] Preferably, in step 2, the area of the copper foam used as the counter electrode is 2 cm×2 cm.
[0014] Preferably, in step 2, the distance between the two electrode sheets is 1 cm.
[0015] Preferably, in step 2, the electrodeposition process uses a DC power supply and is set at a constant cathode current of 0.75 A, and the electrodeposition time is 10 s.
[0016] Preferably, in step three, the specific parameters of the heat treatment are: heating from room temperature to 200° C. over 200 min and keeping the temperature for 2 h, and then naturally cooling to room temperature.
[0017] Compared with the prior art, the present invention has the following beneficial effects: the electrocatalyst prepared by the present invention uses copper foam as a substrate and copper film as an active ingredient, so the raw material cost is relatively low; the present invention only requires pretreatment of the copper foam, and then cathode electrodeposition and heating post-treatment to obtain a finished electrocatalyst without the need for subsequent modification, so the preparation process is simpler; the electrocatalyst prepared by the present invention has the advantages of high electrocatalytic rate, good Faraday efficiency of ammonia production and stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 This is the electron microscope image of Cu / CF;
[0019] Figure 1 (a) is an electron microscope image of Cu / CF at 150 times magnification;
[0020] Figure 1 (b) is the electron microscope image of Cu / CF at 5000 times magnification;
[0021] Figure 1 (c) is an electron microscope image of Cu / CF at 20,000 times magnification;
[0022] Figure 2The X-ray powder diffraction spectra of the newly prepared Cu / CF electrocatalyst and the Cu / CF electrocatalyst after electrocatalytic reduction of nitrate to produce ammonia for 0.5 h are shown in the figure. The standard XRD PDF spectra of Cu2O and Cu are given;
[0023] Figure 3 The Raman spectra of the CF substrate, the newly prepared Cu / CF, and the Cu / CF electrocatalyst after electrocatalytic reduction of nitrate to produce ammonia for 0.5 h. The 400-700 cm -1 The peak is the copper oxide peak;
[0024] Figure 4 Linear sweep voltammetry curves of CF and Cu / CF in 1MKOH and 1000ppmKNO3+1MKOH solutions, respectively, with a scan rate of 0.1Vs -1 ;
[0025] Figure 5 The ammonia production rate and Faradaic efficiency of the electroreduction of nitrate by Cu / CF at different applied potentials. The solution composition was 1000ppm KNO3+1MKOH; the electrolysis time was 0.5h.
[0026] Figure 6 The components (NO3 - 、NO2 - and NH3) concentration changes with time, the solution composition is 500ppmKNO3+1MKOH;
[0027] Figure 7 This is the stability cycle test diagram of Cu / CF for nitrate electroreduction to produce ammonia, the electrolysis potential is -0.4V (vs.RHE);
[0028] Figure 8 is a flow chart of a method according to an embodiment of the present invention;
[0029] Fig. 9 This is a flow chart of the method of Experimental Example 1 of the present invention. DETAILED DESCRIPTION
[0030] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] Please see attached Figure 1 -Attached Fig. 9 , a technical solution provided by the present invention:
[0032] Example:
[0033] A copper electrocatalyst for electrochemically reducing nitrate to produce ammonia comprises a substrate and an active component, wherein the substrate is foamed copper and the active component is a copper film.
[0034] A method for preparing a copper electrocatalyst for electrochemical reduction of nitrate to produce ammonia, comprising the steps of: first, pretreatment of a substrate; second, electrodeposition to generate an active component; and third, heat treatment to obtain the copper electrocatalyst;
[0035] In the above step 1, the copper foam is pretreated to remove the oxide layer and organic matter on the surface. The pretreatment is specifically as follows: immersing the copper foam in 1M HCl for ultrasonic cleaning for 3 minutes, then immersing it in anhydrous ethanol for ultrasonic cleaning for 3 minutes, and finally immersing it in deionized water for ultrasonic cleaning for 3 minutes, wherein the area of the copper foam is 0.5 cm×0.5 cm;
[0036] In the above step 2, the copper foam pretreated in step 1 is taken, and the copper foam is clamped by a platinum electrode clamp and placed in a single-chamber reaction tank filled with an electroplating solution, and a copper foam with an area of 2 cm×2 cm is used as a counter electrode, and the two electrode sheets are kept parallel to each other to perform copper electroplating, and a copper film is generated on the surface of the copper foam; wherein the electroplating solution is composed of: 0.015 M CuSO4+0.15 M K2SO4+0.03 M H2SO4, and the effective volume of the single-chamber reaction tank is 50 ml; the distance between the two electrode sheets is 1 cm; the electroplating process uses a DC power supply and is set to be carried out at a constant cathode current of 0.75 A, and the electroplating time is 10 s;
[0037] In the above step three, the foam copper with the copper film formed on the surface in step two is placed in a beaker filled with deionized water for washing, and then placed in a tubular furnace for heat treatment. After completion of the heat treatment, a three-dimensional porous copper electrocatalyst is obtained, wherein the specific parameters of the heat treatment are: heating from room temperature to 200°C over 200 minutes and keeping warm for 2 hours, and then naturally cooling to room temperature.
[0038] Experimental Example 1:
[0039] In order to verify the electrochemical performance of the three-dimensional porous copper electrocatalyst (Cu / CF) prepared in the example, an electrocatalytic reduction nitrate test experiment was carried out. The experimental method is as follows: Fig. 9 As shown, it specifically includes step 1, preparing an electrochemical performance test experimental device; step 2, electrochemical performance test of electrode materials; step 3, determination of reaction species concentration and performance parameter determination; step 4, analysis of experimental results;
[0040] In the above step 1, a three-electrode electrolytic cell device is used as an experimental device, which is composed of an H-type diaphragm electrolytic cell, a working electrode, a counter electrode, a reference electrode, an electrochemical workstation and a wire. The working electrode is a platinum sheet electrode clip and the three-dimensional porous copper electrocatalyst electrode material prepared in the embodiment, the counter electrode is a platinum sheet electrode, and the reference electrode is a mercury-mercury oxide electrode. The working electrode and the reference electrode are placed in the cathode reaction cell, the counter electrode is placed in the anode reaction cell, and an NR211 perfluorosulfonic acid ion membrane is placed between the two reaction cells to separate them. The three electrodes are fixed through the holes on the electrolytic cell cover;
[0041] In the above step 2, the electrochemical performance test of the three-dimensional porous copper electrocatalyst (Cu / CF) is carried out using the experimental device prepared in step 1. In the electrochemical performance test, linear sweep voltammetry (LSV) test and chronopotentiometry (IT) test are mainly carried out in an H-type electrolytic cell, wherein the cathode pool electrolyte solution of the reaction is 1000ppm KNO3+1M KOH, the anode pool electrolyte solution is 1M KOH, and the volume of the cathode and anode electrolytes is 45mL; in the electrochemical test, all measured potentials are compensated by 80% ohmic drop, magnetic stirring is used during the reaction, the rotation speed is 300 revolutions per minute, and the potential conversion formula is:
[0042] E(vs.RHE)=E(vs.Hg / HgO)+0.069+0.059×pH;
[0043] In the above step 3, a certain amount of the reaction solution in step 2 is taken for color development reaction, and the concentrations of nitrate ions, nitrite ions and ammonia therein are respectively determined by a UV-visible spectrophotometer using a standard curve method, so as to calculate the ammonia production rate and the Faraday efficiency;
[0044] In the above step 4, the experimental data obtained in steps 2 and 3 are analyzed and processed to obtain the following results:
[0045] 1) LSV diagrams of Cu / CF electrocatalyst and CF substrate in 1000ppm KNO3+1M KOH and 1M KOH, respectively. Figure 4 As shown, compared with the behavior in the blank electrolyte (1M KOH), both materials showed obvious reduction current in the electrolyte of 1000ppm KNO3+1M KOH, indicating that both have electrocatalytic reduction activity, but the current of Cu / CF is significantly greater than that of the CF substrate, indicating that the Cu / CF electrocatalyst has a higher activity in the electroreduction of nitrate;
[0046] 2) The ammonia production rate and Faradaic efficiency of the electroreduction of nitrate by Cu / CF at different applied potentials (-0.1 to -0.5 V vs. RHE) are shown in the attached figure. Figure 5As shown in Figure 2, as the potential becomes more negative, the ammonia production rate and FE gradually increase, and the ammonia production rate reaches a maximum value (4.79 mmol h) at -0.4 V (vs. RHE). -1 cm -2 ), the Faraday efficiency reached 70.22%; when the potential continued to shift negatively to -0.5V (vs.RHE), the hydrogen evolution reaction was intense, and a large number of hydrogen bubbles were formed, which damaged the electrode surface to a certain extent, resulting in a decrease in the performance of the latter stage of the electroreduction reaction. Considering the ammonia production rate and the Faraday efficiency, it was concluded that -0.4V (vs.RHE) was the optimal electrolysis potential;
[0047] 3) NO3 in the electrocatalytic reduction process - 、NO2 - The concentration of NH3 changes with time, and the kinetic curve is determined. Figure 6 It can be seen that as the reaction proceeds, NO3 - The concentration of NO2 - The concentration of NH3 gradually increases first, and then begins to decrease after reaching the maximum value, while the concentration of NH3 has been increasing, which is consistent with the characteristics of continuous reaction kinetics, indicating that in the 3h of electrolysis, nitrate is first reduced to nitrite, and then further reduced to ammonia;
[0048] Experimental Example 2:
[0049] In order to test the stability of the three-dimensional porous copper electrocatalyst (Cu / CF) prepared in the example as an electrode material, the experimental device in Experimental Example 1 was used, and 1000 pm KNO3 + 1 MKOH was used as the electrolyte to react continuously at a potential of -0.4 V (vs. RHE) for 3 hours. In order to prevent NO3 from being - The decrease in concentration has an impact on the performance measurement. The electrolyte is replaced every half an hour. After six consecutive electrochemical tests, it can be seen that the ammonia production rate of Cu / CF decreases very little, and FE is relatively stable, indicating that Cu / CF has good stability. The stability cycle test results of Cu / CF are shown in the attached Figure 7 shown.
[0050] Based on the above, the advantages of the present invention are that the present invention uses copper as an electrocatalyst, that is, the substrate is a commercial three-dimensional porous copper foam, and the active component is a copper film, which has the advantage of low raw material cost; the process of the present invention is simple, and only requires pretreatment of the electrode, followed by cathode electrodeposition and heating post-treatment. Since the active component grows directly on the substrate, no subsequent modification is required; the three-dimensional porous copper electrocatalyst prepared by the present invention has a high rate of electrocatalytic nitrate reduction to produce ammonia, and has good Faraday efficiency and stability in producing ammonia.
[0051] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.
Claims
1. A copper electrocatalyst for electrochemical reduction of nitrate to produce ammonia, comprising a substrate and an active component, characterized in that: The substrate is foamed copper, and the active component is a copper film.
2. A method for preparing a copper electrocatalyst for electrochemical reduction of nitrate to produce ammonia, comprising step 1, substrate pretreatment; step 2, electrodeposition to generate active components; step 3, heat treatment to obtain the copper electrocatalyst; characterized in that: In the above step 1, the copper foam is pretreated to remove the oxide layer and organic matter on the surface; In the above step 2, the copper foam pretreated in step 1 is taken, the copper foam is clamped by a platinum electrode clamp and placed in a single-chamber reaction tank filled with an electroplating solution, the copper foam is used as a counter electrode, the two electrode sheets are kept parallel, copper is electrodeposited, and a copper film is formed on the surface of the copper foam; In the above step three, the copper foam with the copper film formed on the surface in step two is placed in a beaker filled with deionized water for cleaning, and then placed in a tubular furnace for heat treatment. After the heat treatment is completed, a three-dimensional porous copper electrocatalyst is obtained.
3. The method for preparing a copper electrocatalyst for electrochemical reduction of nitrate to produce ammonia according to claim 2, characterized in that: In the step 1, the pretreatment is specifically as follows: immersing the copper foam in 1M HCl for ultrasonic cleaning for 3 minutes, then immersing it in anhydrous ethanol for ultrasonic cleaning for 3 minutes, and finally immersing it in deionized water for ultrasonic cleaning for 3 minutes.
4. The method for preparing a copper electrocatalyst for electrochemical reduction of nitrate to produce ammonia according to claim 3, characterized in that: The area of the copper foam is 0.5 cm×0.5 cm.
5. The method for preparing a copper electrocatalyst for electrochemical reduction of nitrate to produce ammonia according to claim 2, characterized in that: In the step 2, the composition of the electroplating solution is: 0.015M CuSO4+0.15MK2SO4+0.03M H2SO4.
6. The method for preparing a copper electrocatalyst for electrochemical reduction of nitrate to produce ammonia according to claim 2, characterized in that: In the step 2, the effective volume of the single-chamber reaction pool is 50 ml.
7. The method for preparing a copper electrocatalyst for electrochemical reduction of nitrate to produce ammonia according to claim 2, characterized in that: In the step 2, the area of the copper foam used as the counter electrode is 2 cm×2 cm.
8. The method for preparing a copper electrocatalyst for electrochemical reduction of nitrate to produce ammonia according to claim 2, characterized in that: In the step 2, the distance between the two electrode sheets is 1 cm.
9. The method for preparing a copper electrocatalyst for electrochemical reduction of nitrate to produce ammonia according to claim 2, characterized in that: In the step 2, the electrodeposition process uses a DC power supply and is set to be performed at a constant cathode current of 0.75 A, and the electrodeposition time is 10 s.
10. The method for preparing a copper electrocatalyst for electrochemical reduction of nitrate to produce ammonia according to claim 2, characterized in that: In the step 3, the specific parameters of the heat treatment are: heating from room temperature to 200° C. over 200 min and keeping the temperature for 2 h, and then naturally cooling to room temperature.
Citation Information
Cited By
Preparation method and application of Al-doped CuO nanosheet electrocatalyst
CN119824460A
A copper-based monatomic alloy electrocatalyst, a preparation method and application thereof