Preparation method and application of polyphenylene sulfide-based composite diaphragm of alkaline electrolytic cell
By generating layered double hydroxide nanoparticles on the polyphenylene sulfide (PPS) membrane, the problem of poor hydrophilicity of PPS membrane in high-temperature alkaline electrolysis environment was solved, thereby improving the membrane performance and increasing the efficiency of hydrogen production from water electrolysis.
Patent Information
- Application Number
- CN202410954986.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-08
AI Technical Summary
Existing polyphenylene sulfide membranes used in alkaline electrolyzers exhibit poor hydrophilicity in high-temperature alkaline electrolysis environments, leading to increased resistance and decreased performance. Furthermore, traditional modification methods are complex and pollute the environment.
By impregnating the polyphenylene sulfide fiber with an alcohol solution of transition metal salt and treating it with an inorganic alkaline solution, it is converted into a layered double hydroxide (LDH), which generates hydrophilic nanoparticles on the surface and interstices of the polyphenylene sulfide fiber, thereby improving the membrane performance.
The modification process was simplified, energy consumption was reduced, the hydrophilicity and mechanical properties of the membrane were improved, and the efficiency of hydrogen production by water electrolysis was enhanced.
Smart Images

Figure CN118910672A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of hydrogen production by alkaline water electrolysis, and specifically relates to a preparation method and application of a polyphenylene sulfide-based composite diaphragm for an alkaline electrolytic cell. Background Art
[0002] With the increasing depletion of traditional fossil energy and the resulting environmental pollution, humans are constantly turning their attention to new clean energy such as solar energy, wind energy, and hydrogen energy. Among them, clean energy represented by hydrogen energy has the advantages of high combustion calorific value, high energy density, and low pollution, and has attracted more and more attention. At present, one of the main ways to obtain hydrogen energy is to produce hydrogen by electrolysis of water. By using H2 as an energy carrier, the electricity generated by renewable energy is stored in the chemical bonds of H2 through the electrochemical cracking of water.
[0003] In 2022, China's electrolyzer shipments will be around 800MW, most of which are alkaline hydrogen production. It is estimated that in 2025, the market size of diaphragms for alkaline water electrolysis hydrogen production equipment in my country will be 840 million, and in 2030 it will reach 2.87 billion, with an annual compound growth rate of 36.67%. Alkaline water electrolysis hydrogen production technology (ALK) has become the mainstream choice for industrial-scale green hydrogen production, but it still has problems such as high unit hydrogen production energy consumption and difficulty in coupling with renewable energy. The key to reducing hydrogen production energy consumption, achieving electric-hydrogen coupling, improving hydrogen production efficiency and ensuring safety lies in the key component of ALK hydrogen production equipment - the diaphragm. The ohmic resistance and conductivity of the diaphragm are directly linked to the hydrogen production energy consumption, while the air tightness of the diaphragm is closely related to the safety of hydrogen production. The diaphragm occupies a very important position in the electrolyzer, and its main functions include three aspects: (1) separating the cathode and anode to form cathode and anode chambers to prevent short circuits; (2) avoiding mixing of gas products at both electrodes; and (3) transferring hydroxide ions from the cathode to the anode. Therefore, the ideal membrane material should have the following characteristics: (1) good ion conductivity, high porosity, and low resistivity; (2) high gas barrier properties, high hydrophilicity, and high corrosion resistance; (3) thin thickness, small pore size, high mechanical strength, and good dimensional stability; (4) low cost and long service life.
[0004] As asbestos diaphragms have the characteristics of large specific surface area, good conductivity, corrosion resistance and low cost, so they have been widely used in early electrolytic water production. However, asbestos diaphragms are prone to expansion after the electrolytic cell is powered on, so that the asbestos fibers fill the gap between the electrode and the diaphragm, making the diaphragm susceptible to erosion by the gas released by the electrode, causing wear and tear, shortening the service life of the diaphragm, and even requiring the cell to be stopped and replaced, affecting normal production. Secondly, asbestos can be split into very fine fibers during mining, processing, production and use. After being released, these fine fibers can float in the air for a long time, accumulate in the body through the respiratory tract, and induce cancer in severe cases.
[0005] Polyphenylene sulfide (PPS) is a high-performance special engineering material that can maintain stable performance under alkaline and high temperature conditions. Therefore, it is used to prepare alkaline hydrogen production diaphragms. In the iteration of material systems and commercial exploration, PPS diaphragms have been valued by the market and have become the most widely used material. At present, PPS diaphragms have firmly occupied more than 95% of the domestic market share. However, due to the strong hydrophobicity of polymer materials, they cause large impedance during use and cannot be directly used as water electrolysis diaphragms. Generally, they need to be treated by high-temperature sulfonation in 98-99% concentrated sulfuric acid to form a hydrophilic surface so that the alkali solution can have sufficient infiltration of the material. However, the hydrophilic groups formed after surface modification are difficult to withstand the high-temperature alkaline electrolysis environment for a long time, and the performance of the diaphragm is significantly reduced during use. At the same time, the use of high-concentration sulfuric acid poses severe challenges to large-scale industrial production and poses a serious threat to the environment.
[0006] For example, patent CN 101372752 B discloses a method for preparing a needle-punched nonwoven polyphenylene sulfide diaphragm, which is made of a nonwoven fabric with a certain strength by selecting PPS fiber, and sulfonating it in 90-98% H2SO4 for 20-40 minutes to improve its hydrophilicity; but this method still has the disadvantages of complicated steps and harm to the environment; patent CN 202410068488.5 improves its hydrophilicity by vacuum plasma surface treatment of PPS diaphragm in argon atmosphere, and then immerses it in a solution containing inorganic materials to obtain a diaphragm with high bubble point and low surface resistance, but its treatment process is complicated, and plasma treatment is required under a vacuum pressure of 30-60Pa, which is not conducive to large-scale production. Therefore, how to improve the hydrophilicity of the surface of PPS material and prepare an alkaline electrolyzer diaphragm with good performance through a simple, efficient, green and environmentally friendly method is an urgent problem to be solved in the field of alkaline water electrolysis hydrogen production. Summary of the invention
[0007] The purpose of the present invention is to provide a preparation method and application of a polyphenylene sulfide-based composite membrane for an alkaline electrolytic cell in view of the poor performance of the existing polyphenylene sulfide membrane for an alkaline electrolytic cell. The method soaks the hydrophobic polyphenylene sulfide membrane in an alcohol solution of a transition metal salt, and the organic alcohol can more effectively promote the diffusion of transition metal salt ions, and can ensure that the transition metal salt ions enter the fiber gap more effectively, thereby converting into a layered double hydroxide (LDH). The present invention does not use chemical reagents such as strong acids and strong oxidants throughout the entire process, is simple and efficient, does not have high energy consumption steps, is clean and pollution-free, and effectively protects the environment.
[0008] The technical solution of the present invention is:
[0009] A method for preparing a polyphenylene sulfide-based composite diaphragm for an alkaline electrolytic cell, the method comprising the following steps:
[0010] (1) immersing the hydrophobic polyphenylene sulfide membrane in a transition metal salt solution for 0.1-1 h, and then rinsing with alcohol;
[0011] Wherein, the concentration of transition metal salt is 0.15-0.45M;
[0012] (2) soaking the obtained polyphenylene sulfide membrane with transition metal salt ions in an inorganic alkali solution for 10-30 minutes, and then rinsing with alcohol;
[0013] Wherein, the concentration of the inorganic alkali solution is 0.1-0.2M;
[0014] (3) drying the obtained diaphragm in an oven at 60-80° C. for 12-24 hours, thereby obtaining a polyphenylene sulfide-based composite diaphragm for an alkaline electrolytic cell;
[0015] The transition metal salt is one of nickel nitrate, iron nitrate, cobalt nitrate, and ferrous sulfate, or a combination of the two. When two transition metal salts are added, the molar ratio thereof is 5:1-1:5.
[0016] The solvents of the transition metal salt solution and the inorganic alkali solution are the same, namely, alcohol.
[0017] The alcohol used for rinsing in steps (1) and (2) is the same as that used in the transition metal salt solution and the inorganic alkali solution.
[0018] The inorganic base is potassium hydroxide or sodium hydroxide.
[0019] The alcohol is ethanol, methanol or isopropanol.
[0020] The infiltration temperature in step (1) and step (2) is 25-60°C, preferably 60°C.
[0021] The polyphenylene sulfide-based composite diaphragm of the alkaline electrolyzer prepared by the method is used for producing hydrogen by alkaline water electrolysis.
[0022] The essential features of the present invention are:
[0023] The present invention is different from the previous methods of high temperature sulfonation treatment of polyphenylene sulfide diaphragm in 98-99% concentrated sulfuric acid. Instead, the polyphenylene sulfide diaphragm is directly treated in an alcohol solution of a transition metal salt at 25-60°C to expand the internal fiber gap while attaching transition salt ions on the fiber surface and in the gap through a diffusion process, and then reacting in an alcohol solution of an inorganic base at 25-60°C to convert the transition metal salt ions into layered double hydroxides (LDH), and then drying in a 60-80°C oven to obtain an alkaline electrolytic cell polyphenylene sulfide-based composite diaphragm. The generation of LDH on the fiber surface and between the gaps not only improves the hydrophilicity of the diaphragm, reduces the energy consumption caused by the hydrophobic characteristics of polyphenylene sulfide, but also accelerates the transmission process of hydroxide ions in the water electrolysis process, thereby improving the overall performance of the diaphragm. The resulting diaphragm can be used in devices such as alkaline water electrolysis hydrogen production to reduce energy consumption in the water electrolysis process.
[0024] The beneficial effects of the present invention are:
[0025] (1) Due to the strong hydrophobicity of polymer materials, the electrolyte is hindered from wetting the inside of the membrane during use, causing the membrane resistance to increase. At the same time, hydrophobic substances are easily accumulated on the membrane surface, causing membrane surface pollution. The traditional hydrophobic modification method requires high-temperature sulfonation in 98-99% concentrated sulfuric acid to form a hydrophilic surface. However, the hydrophilic groups formed after surface modification are difficult to withstand the high-temperature alkaline electrolysis environment for a long time, and the performance of the diaphragm is significantly reduced during use. At the same time, the use of high-concentration sulfuric acid poses a severe challenge to large-scale industrial production and poses a serious threat to the environment. However, this method does not use chemical reagents such as strong acids and strong oxidants throughout the process. It is simple, efficient, clean and pollution-free, and effectively protects the environment. (2) The use of alcohol solution can increase the gap between polyphenylene sulfide fibers, which is beneficial to the entry of transition metal salt ions, so that the inside of the polyphenylene sulfide diaphragm has a high specific surface area, and the hydrophilic particles grow evenly and are not easy to fall off. The generation of hydrophilic nanoparticles on the fiber surface and in the fiber gap can not only improve the overall hydrophilicity of the diaphragm, but also improve the mechanical properties, especially the high temperature resistance. Secondly, the generation of LDH accelerates the transport of hydroxyl radicals during water electrolysis and improves the water electrolysis performance of the overall electrolyzer. Figure 4 It can be seen that compared with the 0.8 mm hydrophobic polyphenylene sulfide diaphragm, the performance of the 0.8 mm hydrophilic polyphenylene sulfide diaphragm electrolyzer was significantly improved after modification, and it can reach 466 mA cm at a working voltage of 2 V. -2 The current density is much higher than 217 mA cm of 0.8 mm hydrophobic polyphenylene sulfide membrane. -2 of current density. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1This is a process flow chart of the preparation of the polyphenylene sulfide-based composite diaphragm prepared in Example 1.
[0027] Figure 2 is a comparison diagram of the morphology of the polyphenylene sulfide-based composite membrane prepared in Example 1 before and after preparation;
[0028] Figure 3 This is a field emission electron scanning electron micrograph of the polyphenylene sulfide-based composite membrane prepared in Example 1.
[0029] Figure 4 This is a performance test diagram of the polyphenylene sulfide-based composite diaphragm prepared in Example 1 with a fixture. DETAILED DESCRIPTION
[0030] The following examples further illustrate the content of the present invention, but should not be construed as limiting the present invention. Without departing from the spirit and essence of the present invention, modifications and substitutions made to the methods, steps or conditions of the present invention all belong to the scope of the present invention.
[0031] Unless otherwise specified, the technical means used in the examples are conventional means well known to those skilled in the art.
[0032] The process steps of the present invention are as follows Figure 1 As shown, the steps include infiltration with an alcohol solution of a transition metal salt, alcohol rinsing, infiltration with an alcohol solution of an inorganic base, alcohol rinsing, oven drying, and collection.
[0033] The hydrophobic polyphenylene sulfide diaphragm involved in the present invention is a known material, specifically 0.8 mm thick, purchased from Tianjin Jinlun New Material Technology Co., Ltd., model GY-450. But not limited thereto.
[0034] Example 1
[0035] (1) The area is 49cm 2 1. A 0.8 mm thick hydrophobic polyphenylene sulfide membrane was immersed in a 60°C transition metal salt ethanol solution (the transition metal salts were nickel nitrate and ferrous sulfate, the molar ratio of the two was 1:1, and the concentration was 0.15 M) for 0.5 h, and then rinsed in new ethanol to remove excess transition metal salt ions on the surface (wash until the transition metal salt ions attached to the surface are not detached);
[0036] (2) placing the obtained polyphenylene sulfide diaphragm with Ni and Fe ions attached in a 0.1 M potassium hydroxide ethanol solution at 60° C. for 30 min, so that all attached Ni and Fe ions participate in the reaction, and rinsing in new ethanol to remove excess alkaline solution on the surface;
[0037] (3) drying the obtained diaphragm in an oven at 80° C. for 24 h, thereby obtaining a polyphenylene sulfide-based composite diaphragm for an alkaline electrolytic cell;
[0038] The morphology of the obtained diaphragm before and after preparation is as follows Figure 2 As shown, Figure 2 As shown in (left), the initial hydrophobic membrane is milky white in color, which means that there are no particles attached to the fiber gaps and fiber surfaces. Figure 2 (Right) As shown, its color is yellow-brown, which is consistent with the color of the grown LDH nanoparticles, which successfully proves the successful growth of LDH on the surface and inside of the membrane.
[0039] The field emission electron scanning electron microscopy results of the surface and gap of the obtained diaphragm fiber are as follows: Figure 3 shown by Figure 3 It can be seen that there are obvious nanoparticles attached to the surface of polyphenylene sulfide fibers, and the particle size is uniform, which further proves the effectiveness of the method.
[0040] The prepared diaphragm was assembled into a fixture and the electrolysis performance test was carried out at a flow rate of 40 mL / min using a blue battery test system, 80°C, 30% KOH solution as the electrolyte, and Raney nickel mesh as the cathode and anode catalyst. The test results are shown in the figure. Figure 4 shown by Figure 4 It can be seen that compared with the 0.8 mm hydrophobic polyphenylene sulfide diaphragm, the performance of the 0.8 mm hydrophilic polyphenylene sulfide diaphragm electrolyzer was significantly improved after modification, and it can reach 466 mA cm at a working voltage of 2 V. -2 The current density is much higher than 217 mA cm of 0.8 mm hydrophobic polyphenylene sulfide membrane. -2 The above analysis shows that the growth of hydrophilic layered double hydroxide nanoparticles on the surface and gaps of hydrophobic polyphenylene sulfide diaphragm fibers can significantly improve the hydrophilicity of the diaphragm, thereby enhancing its water electrolysis performance.
[0041] Example 2
[0042] (1) The area is 49cm 2 , a 0.8 mm thick hydrophobic polyphenylene sulfide membrane was immersed in a 60°C transition metal salt isopropanol solution (the transition metal salt is nickel nitrate, with a concentration of 0.15 M) for 0.5 h, and then rinsed in new isopropanol to remove excess transition metal salt ions on the surface
[0043] (2) placing the obtained polyphenylene sulfide diaphragm with Ni ions attached in a 0.1 M potassium hydroxide isopropanol solution at 60° C. for 30 min, so that all attached Ni ions participate in the reaction, and rinsing in new isopropanol to remove excess alkaline solution on the surface;
[0044] (3) drying the obtained diaphragm in an oven at 80° C. for 24 h, thereby obtaining a polyphenylene sulfide-based composite diaphragm for an alkaline electrolytic cell;
[0045] Example 3
[0046] (1) The area is 49cm 2 , a 0.8 mm thick hydrophobic polyphenylene sulfide membrane was immersed in a 60°C transition metal salt methanol solution (the transition metal salt is ferrous sulfate, with a concentration of 0.15 M) for 1 h, and then rinsed in new methanol to remove excess transition metal salt ions on the surface
[0047] (2) placing the obtained polyphenylene sulfide diaphragm with Fe ions attached in a 0.15 M sodium hydroxide methanol solution at 60° C. for reaction for 30 min, so that all attached Fe ions participate in the reaction, and rinsing in new methanol to remove excess alkaline solution on the surface;
[0048] (3) drying the obtained diaphragm in an oven at 80° C. for 24 h, thereby obtaining a polyphenylene sulfide-based composite diaphragm for an alkaline electrolytic cell;
[0049] Example 4
[0050] (1) The area is 49cm 2 , a 0.8 mm thick hydrophobic polyphenylene sulfide membrane was immersed in an ethanol solution of transition metal salts (the transition metal salts were nickel nitrate and iron nitrate, the molar ratio of the two was 2:1, and the concentrations were 0.3 M and 0.15 M) at room temperature (25°C) for 1 hour, and then rinsed in new ethanol to remove excess transition metal salt ions on the surface
[0051] (2) placing the obtained polyphenylene sulfide diaphragm with Ni and Fe ions attached in a 0.1 M potassium hydroxide ethanol solution at room temperature (25° C.) for 30 minutes, so that all attached Ni and Fe ions participate in the reaction, and rinsing in new ethanol to remove excess alkaline solution on the surface;
[0052] (3) drying the obtained diaphragm in an oven at 80° C. for 24 h, thereby obtaining a polyphenylene sulfide-based composite diaphragm for an alkaline electrolytic cell;
[0053] Example 5
[0054] (1) The area is 49cm 2 , a 0.8 mm thick hydrophobic polyphenylene sulfide membrane was immersed in a 60°C transition metal salt isopropanol solution (the transition metal salts are cobalt nitrate and iron nitrate, the molar ratio of the two is 1:2, and the concentrations are 0.15M and 0.3M) for 0.5 h, and then rinsed in new isopropanol to remove excess transition metal salt ions on the surface
[0055] (2) placing the obtained polyphenylene sulfide diaphragm with attached Co and Fe ions in a 0.2 M sodium hydroxide isopropanol solution at 60° C. for reaction for 30 min, so that all attached Co and Fe ions participate in the reaction, and rinsing in new isopropanol to remove excess alkaline solution on the surface;
[0056] (3) drying the obtained diaphragm in an oven at 80° C. for 24 h, thereby obtaining a polyphenylene sulfide-based composite diaphragm for an alkaline electrolytic cell;
[0057] Example 6
[0058] (1) The area is 49cm 2 , a 0.8 mm thick hydrophobic polyphenylene sulfide membrane was immersed in a 60°C transition metal salt ethanol solution (the transition metal salts were nickel nitrate and ferrous sulfate, the molar ratio of the two was 3:1, the concentrations were 0.3M and 0.1M) for 0.5 h, and then rinsed in new ethanol to remove excess transition metal salt ions on the surface
[0059] (2) placing the obtained polyphenylene sulfide diaphragm with Ni and Fe ions attached in a 0.1 M sodium hydroxide ethanol solution at 60° C. for reaction for 30 min, so that all attached Ni and Fe ions participate in the reaction, and rinsing in new ethanol to remove excess alkaline solution on the surface;
[0060] (3) The obtained diaphragm was dried in an oven at 80° C. for 24 h to obtain a polyphenylene sulfide-based composite diaphragm for an alkaline electrolytic cell; Comparative Example 1
[0061] (1) The area is 49cm 2 The hydrophobic polyphenylene sulfide membrane with a thickness of 0.8 mm was ultrasonically cleaned in ethanol to remove the stains on its surface. After that, the prepared membrane was assembled into a fixture and the electrolysis performance was tested at a flow rate of 40 mL / min using a blue battery test system, 80°C, 30% KOH solution as the electrolyte, and Raney nickel mesh as the cathode and anode catalyst. The test results are as follows Figure 4 As shown in the figure, compared with the modified 0.8 mm hydrophilic polyphenylene sulfide membrane, the 0.8 mm hydrophobic polyphenylene sulfide membrane electrolyzer only reached 217 mA cm at a working voltage of 2 V. -2 The current density is much lower than that of the modified 0.8 mm hydrophilic polyphenylene sulfide diaphragm electrolyzer (466 mA cm -2 @2V). The reason why the hydrophobic polyphenylene sulfide diaphragm electrolyzer has poor performance may be that the polymer material is highly hydrophobic, which hinders the electrolyte from penetrating into the membrane during use, causing the membrane resistance to increase, thereby resulting in a large performance loss.
[0062] Matters not covered by the present invention are known technologies.
Claims
1. A method for preparing a polyphenylene sulfide-based composite diaphragm for an alkaline electrolytic cell, characterized in that the method comprises the following steps: (1) immersing the hydrophobic polyphenylene sulfide membrane in a transition metal salt solution for 0.1-1 h, and then rinsing with alcohol; Wherein, the concentration of transition metal salt is 0.15-0.45M; (2) soaking the obtained polyphenylene sulfide membrane with transition metal salt ions in an inorganic alkali solution for 10-30 minutes, and then rinsing with alcohol; Wherein, the concentration of the inorganic alkali solution is 0.1-0.2M; (3) drying the obtained diaphragm in an oven at 60-80° C. for 12-24 hours, thereby obtaining a polyphenylene sulfide-based composite diaphragm for an alkaline electrolytic cell; The transition metal salt is one of nickel nitrate, iron nitrate, cobalt nitrate, and ferrous sulfate, or a combination of the two, wherein when two transition metal salts are added, the molar ratio thereof is 5:1-1:5; The solvents of the transition metal salt solution and the inorganic alkali solution are the same, namely, alcohol.
2. The method for preparing a polyphenylene sulfide-based composite diaphragm for an alkaline electrolytic cell according to claim 1, characterized in that The alcohol used for rinsing in steps (1) and (2) is the same as that used in the transition metal salt solution and the inorganic alkali solution.
3. The method for preparing a polyphenylene sulfide-based composite diaphragm for an alkaline electrolytic cell according to claim 1, wherein the inorganic base is potassium hydroxide or sodium hydroxide.
4. The method for preparing a polyphenylene sulfide-based composite diaphragm for an alkaline electrolytic cell according to claim 1, characterized in that The alcohol is ethanol, methanol or isopropanol.
5. The method for preparing a polyphenylene sulfide-based composite diaphragm for an alkaline electrolytic cell according to claim 1, characterized in that The infiltration temperature in step (1) and step (2) is 25-60°C.
6. Use of the method as claimed in claim 1 for preparing a polyphenylene sulfide-based composite diaphragm for an alkaline electrolytic cell, characterized in that it is used for producing hydrogen by alkaline electrolysis of water.