Additive for electrolytic copper foil, electrolyte and preparation method of electrolytic copper foil

By using additives for electrolytic copper foils of sodium polydisulfonate, chlorine, methylene blue, octylphenol polyethylene glycol ether, molybdenum and zinc in lithium secondary batteries, the problem of electrolytic copper foil fracture has been solved and improved The capacity retention rate and life of lithium secondary batteries achieve higher battery performance and reliability.

CN118910684APending Publication Date: 2024-11-08SHANDONG JINBAO ELECTRONICS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411328098.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-24
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The electrolytic copper foil in lithium secondary batteries is prone to break during charging and discharging, resulting in low capacity retention and short life, affecting the performance and reliability of the secondary battery.

Method used

Using additives for electrolytic copper foils containing sodium polydisulfonate, chlorine, methylene blue, octylphenol polyethylene glycol ether, molybdenum and zinc, to increase copper by controlling the intake and grain size of molybdenum-zinc alloy. The breaking energy and cycle life of the foil.

Benefits of technology

It significantly improves the breaking energy and cycle life of the electrolytic copper foil, prevents the copper foil from breaking in high-temperature processes or abnormal conditions, and improves the safety and cycle life characteristics of the secondary battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005056008270000031
    Figure BDA0005056008270000031
  • Figure BDA0005056008270000091
    Figure BDA0005056008270000091
  • Figure BDA0005056008270000101
    Figure BDA0005056008270000101
Patent Text Reader

Abstract

The invention relates to the technical field of electrolytic copper foils, in particular to an additive for an electrolytic copper foil, an electrolyte and a preparation method of the electrolytic copper foil. The additive for the electrolytic copper foil, provided by the invention, comprises the following components: sodium dithiodipropane sulfonate, chlorine, methylene blue, octylphenol polyethylene glycol ether, molybdenum and zinc. The invention further provides an electrolyte for the electrolytic copper foil. Each liter of the electrolyte comprises 5 to 30 milligrams of sodium dithiodipropane sulfonate, 10 to 40 milligrams of chlorine, 4 to 20 milligrams of methylene blue, 10 to 50 milligrams of octylphenol polyethylene glycol ether, 10 to 300 milligrams of molybdenum and 50 to 800 milligrams of zinc. According to the electrolytic copper foil prepared through the method, the fracture energy is improved, and fracture of the copper foil in the using process is avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of electrolytic copper foil, and in particular to an additive for electrolytic copper foil, an electrolyte and a method for preparing the electrolytic copper foil. Background Art

[0002] A secondary battery is a type of energy converter that converts electrical energy into chemical energy and stores it. When electricity is needed, the chemical energy is converted back into electrical energy to generate electricity. Since secondary batteries can be recharged repeatedly, they are also called rechargeable batteries. Among such secondary batteries, lithium secondary batteries are able to store a relatively large amount of energy relative to their size and weight. In the field of information and communication equipment that emphasizes portability and mobility, lithium secondary batteries are preferred, and their application range is also expanding to energy storage devices for hybrid vehicles and electric vehicles.

[0003] Lithium secondary batteries are repeatedly used in a cycle of charge and discharge. When a device is operated with a fully charged lithium secondary battery, the lithium secondary battery should have a higher charge / discharge capacity to increase the operating time of the device. Therefore, continuous research is required to meet the growing demand for the charge / discharge capacity of lithium secondary batteries.

[0004] A lithium secondary battery includes a negative electrode collector made of copper foil. Among copper foils, electrolytic copper foil is widely used as a negative electrode collector of a lithium secondary battery. As the demand for lithium secondary batteries increases, especially the demand for lithium secondary batteries with high capacity, high efficiency and high quality increases, it is necessary to develop an electrolytic copper foil that can improve the characteristics of lithium secondary batteries, especially a copper foil that can ensure the high capacity and capacity retention rate of lithium secondary batteries.

[0005] On the other hand, the thinner the copper foil is, the more active material can be contained in the same space, thereby increasing the capacity of the secondary battery. However, as the copper foil becomes thinner, it is easy to break during the copper foil manufacturing and battery manufacturing process.

[0006] Although the secondary battery has a sufficiently high charge / discharge capacity, if the charge / discharge capacity of the secondary battery decreases rapidly with the charge / discharge cycle (i.e., if the capacity retention rate is low or the life is short), the secondary battery needs to be replaced frequently, which will waste costs and resources economically and environmentally. As one of the reasons for the reduction in the capacity retention rate of the secondary battery, as the secondary battery is repeatedly charged / discharged, the negative electrode collector will shrink / expand, and at this time, the electrolytic copper foil and the negative electrode material that are tightly attached will be partially peeled off during charging and discharging, and the stress during expansion and contraction is concentrated on the peeled part, which is also easy to cause the copper foil to break. Summary of the invention

[0007] In order to solve the above technical problems existing in the prior art, the present invention provides an additive for electrolytic copper foil, an electrolyte and a method for preparing the electrolytic copper foil.

[0008] The technical solution of the present invention to solve the above technical problems is as follows:

[0009] The first aspect of the present invention is to provide an additive for electrolytic copper foil, comprising the following components:

[0010] Sodium polydisulfide bispropane sulfonate, chlorine, methylene blue, octylphenol polyglycol ether, molybdenum, zinc.

[0011] The beneficial technical effects of the additive for electrolytic copper foil of the present invention are as follows: by adding sodium polydisulfide dipropane sulfonate as a brightener, the surface of the coating is given gloss and a fine coating is obtained; octylphenol polyglycol ether as a non-ionic surfactant can make the copper layer uniformly electroplated during the generation process, preventing the roughness of the electrolytic copper foil from suddenly increasing and causing the strength of the copper foil to decrease; molybdenum and zinc are added at the same time, and the molybdenum-zinc alloy is taken into the copper foil during electrolytic precipitation, so that the changes in the grain size and crystal structure of the copper foil are minimized, and the electrolytic copper foil and the negative electrode material are prevented from being broken due to local peeling during battery charging / discharging, thereby improving the life of the battery; in addition, chlorine is added to the electrolyte in order to utilize the specific adsorption of chlorine to control the amount of molybdenum and zinc alloy taken into the copper foil. If the amount of molybdenum and zinc alloy taken into the copper foil is too much, the conductivity of the copper foil will be reduced, while if the amount taken is too little, the effect of improving the fracture energy cannot be achieved; methylene blue is a dye-type leveling agent, which acts synergistically with chlorine and helps to obtain a more uniform and better quality copper coating in electroplating.

[0012] On the basis of the above technical solution, the present invention can also make the following improvements:

[0013] Further, the octylphenol polyglycol ether has the following structural formula:

[0014]

[0015] Among them, n=10-22.

[0016] Furthermore, the chlorine is taken from chloride, the molybdenum is taken from molybdate, and the zinc is taken from zinc sulfate.

[0017] Furthermore, the chloride is selected from any one of hydrogen chloride, potassium chloride and ammonium chloride; and the molybdate is selected from any one of sodium molybdate, potassium molybdate and ammonium molybdate.

[0018] The second aspect of the present invention is to provide an electrolyte for electrolytic copper foil using the above-mentioned additive for electrolytic copper foil, wherein each liter of the electrolyte contains: 5-30 mg of sodium polydipropylene glycol disulfide, 10-40 mg of chlorine, 4-20 mg of methylene blue, 10-50 mg of octylphenol polyglycol ether, 10-300 mg of molybdenum, and 50-800 mg of zinc.

[0019] By limiting the addition amount of each component in the electrolyte as above, the fracture energy of the prepared electrolytic copper foil is greatly improved. Even if the secondary battery undergoes a high-temperature process during manufacturing or operates under an abnormally high temperature state, the copper foil can continuously maintain quality reliability without breaking, and exhibits excellent cycle life characteristics and safety when used in secondary batteries.

[0020] On the basis of the above technical solution, the present invention can also make the following improvements:

[0021] Furthermore, each liter of the electrolyte contains: 10-25 mg of sodium polydisulfide dipropane sulfonate, 15-30 mg of chlorine, 6-18 mg of methylene blue, 20-40 mg of octylphenol polyglycol ether, 20-250 mg of molybdenum, and 40-700 mg of zinc.

[0022] Furthermore, each liter of the electrolyte contains: 12-22 mg of sodium polydisulfide propane sulfonate, 18-25 mg of chlorine, 8-15 mg of methylene blue, 25-35 mg of octylphenol polyglycol ether, 100-200 mg of molybdenum, and 200-400 mg of zinc.

[0023] Furthermore, the electrolyte is a sulfuric acid-copper sulfate electrolyte, and the molybdate and zinc sulfate are both added to the sulfuric acid-copper sulfate electrolyte in the form of aqueous solutions.

[0024] Furthermore, the copper ion concentration in the sulfuric acid-copper sulfate electrolyte is 85-120 g / L, and the sulfuric acid concentration is 90-120 g / L.

[0025] Another aspect of the present invention is to provide a method for preparing an electrolytic copper foil using the above-mentioned electrolytic copper foil electrolyte, comprising the following steps:

[0026] (1) The electrolyte is fed into a foil machine to produce raw foil, and the electrolysis temperature is controlled to be 50-60°C and the current density is 50-70A / dm 2 ;

[0027] (2) Chromate treatment of raw foil, potassium dichromate concentration of 20-30g / L, temperature of 20-40℃, current density of 5-8A / dm 2 The electroplating time is 6-8 seconds, which gives the electrolytic copper foil corrosion resistance.

[0028] Compared with the prior art, the present invention has the following technical effects:

[0029] The electrolytic copper foil prepared by the present invention has greatly improved fracture energy. Even if the secondary battery undergoes a high-temperature process during manufacturing or operates under an abnormally high temperature state, the copper foil can continuously maintain quality reliability without breaking, and exhibits excellent cycle life characteristics and safety when used in secondary batteries. DETAILED DESCRIPTION

[0030] The following specific embodiments illustrate the implementation of the present invention, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. Although the description of the present invention will be introduced in conjunction with the preferred embodiment, this does not mean that the features of this invention are limited to this implementation. On the contrary, the purpose of introducing the invention in conjunction with the implementation is to cover other options or modifications that may extend based on the claims of the present invention. In order to provide a deep understanding of the present invention, the following description will include many specific details. The present invention can also be implemented without using these details. In addition, in order to avoid confusion or blurring the focus of the present invention, some specific details will be omitted in the description. It should be noted that the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.

[0031] Example 1

[0032] The electrolyte for electrolytic copper foil of this embodiment contains: 17 mg of sodium polydipropane disulfide sulfonate, 22 mg of chlorine, 12 mg of methylene blue, 30 mg of octylphenol polyglycol ether, 150 mg of molybdenum and 300 mg of zinc per liter of sulfuric acid-copper sulfate electrolyte;

[0033] Wherein, chlorine is taken from hydrogen chloride, molybdenum is taken from sodium molybdate, and zinc is taken from zinc sulfate. Sodium molybdate and zinc sulfate are added to sulfuric acid-copper sulfate electrolyte in the form of aqueous solution. The copper ion concentration in the sulfuric acid-copper sulfate electrolyte is 90g / L, and the sulfuric acid concentration is 110g / L.

[0034] The preparation method of the electrolytic copper foil of this embodiment is as follows: the above electrolyte is fed into a foil machine, the electrolysis temperature is controlled to be 55°C, the current density is 60A / dm 2 The raw foil is then chromated at a concentration of 25 g / L potassium dichromate, a temperature of 30 °C, and a current density of 6 A / dm 2 The electroplating time is 7 seconds, and the electrolytic copper foil with a foil thickness of 6μm is produced.

[0035] Example 2

[0036] The electrolyte for electrolytic copper foil of this embodiment contains: 12 mg of sodium polydipropane disulfide sulfonate, 18 mg of chlorine, 8 mg of methylene blue, 25 mg of octylphenol polyglycol ether, 100 mg of molybdenum and 200 mg of zinc per liter of sulfuric acid-copper sulfate electrolyte;

[0037] Wherein, chlorine is taken from potassium chloride, molybdenum is taken from potassium molybdate, and zinc is taken from zinc sulfate. Potassium molybdate and zinc sulfate are added to sulfuric acid-copper sulfate electrolyte in the form of aqueous solution. The copper ion concentration in the sulfuric acid-copper sulfate electrolyte is 90g / L and the sulfuric acid concentration is 110g / L.

[0038] The preparation method of the electrolytic copper foil of this embodiment is as follows: the above electrolyte is fed into a foil machine, the electrolysis temperature is controlled to be 55°C, the current density is 60A / dm 2 The raw foil is then chromated at a concentration of 25 g / L potassium dichromate, a temperature of 30 °C, and a current density of 6 A / dm 2 The electroplating time is 7 seconds, and the electrolytic copper foil with a foil thickness of 8μm is produced.

[0039] Example 3

[0040] The electrolyte for electrolytic copper foil of this embodiment contains 22 mg of sodium polydipropane disulfide sulfonate, 25 mg of chlorine, 15 mg of methylene blue, 35 mg of octylphenol polyglycol ether, 200 mg of molybdenum and 400 mg of zinc per liter of sulfuric acid-copper sulfate electrolyte;

[0041] Wherein, chlorine is taken from ammonium chloride, molybdenum is taken from ammonium molybdate, and zinc is taken from zinc sulfate. Ammonium molybdate and zinc sulfate are added to sulfuric acid-copper sulfate electrolyte in the form of aqueous solution. The copper ion concentration in the sulfuric acid-copper sulfate electrolyte is 90g / L and the sulfuric acid concentration is 110g / L.

[0042] The preparation method of the electrolytic copper foil of this embodiment is as follows: the above electrolyte is fed into a foil machine, the electrolysis temperature is controlled to be 55°C, the current density is 60A / dm 2 The raw foil is then chromated at a concentration of 25 g / L potassium dichromate, a temperature of 30 °C, and a current density of 6 A / dm 2 The electroplating time is 7 seconds, and the electrolytic copper foil with a foil thickness of 9μm is produced.

[0043] Example 4

[0044] The electrolyte for electrolytic copper foil of this embodiment contains: 15 mg of sodium polydipropane disulfide sulfonate, 24 mg of chlorine, 14 mg of methylene blue, 30 mg of octylphenol polyglycol ether, 170 mg of molybdenum and 220 mg of zinc per liter of sulfuric acid-copper sulfate electrolyte;

[0045] Wherein, chlorine is taken from hydrogen chloride, molybdenum is taken from potassium molybdate, and zinc is taken from zinc sulfate. Potassium molybdate and zinc sulfate are added to sulfuric acid-copper sulfate electrolyte in the form of aqueous solution. The copper ion concentration in the sulfuric acid-copper sulfate electrolyte is 90g / L and the sulfuric acid concentration is 110g / L.

[0046] The preparation method of the electrolytic copper foil of this embodiment is as follows: the above electrolyte is fed into a foil machine, the electrolysis temperature is controlled to be 55°C, the current density is 60A / dm 2 The raw foil is then chromated at a concentration of 25 g / L potassium dichromate, a temperature of 30 °C, and a current density of 6 A / dm 2 The electroplating time is 7 seconds, and an electrolytic copper foil with a foil thickness of 10μm is produced.

[0047] Example 5

[0048] The electrolyte for electrolytic copper foil of this embodiment contains: 13 mg of sodium polydipropane disulfide sulfonate, 20 mg of chlorine, 10 mg of methylene blue, 28 mg of octylphenol polyglycol ether, 120 mg of molybdenum and 380 mg of zinc per liter of sulfuric acid-copper sulfate electrolyte;

[0049] Among them, chlorine is taken from potassium chloride, molybdenum is taken from ammonium molybdate, and zinc is taken from zinc sulfate. Ammonium molybdate and zinc sulfate are added to sulfuric acid-copper sulfate electrolyte in the form of aqueous solution. The copper ion concentration in the sulfuric acid-copper sulfate electrolyte is 90g / L and the sulfuric acid concentration is 110g / L.

[0050] The preparation method of the electrolytic copper foil of this embodiment is as follows: the above electrolyte is fed into a foil machine, the electrolysis temperature is controlled to be 55°C, the current density is 60A / dm 2 The raw foil is then chromated at a concentration of 25 g / L potassium dichromate, a temperature of 30 °C, and a current density of 6 A / dm 2 The electroplating time is 7 seconds, and the electrolytic copper foil with a foil thickness of 8μm is produced.

[0051] Comparative Example 1

[0052] The electrolyte of this comparative example contains, per liter of sulfuric acid-copper sulfate electrolyte: 17 mg of sodium polydisulfide dipropane sulfonate, 22 mg of chlorine, 30 mg of octylphenol polyglycol ether, 150 mg of molybdenum and 300 mg of zinc;

[0053] Wherein, chlorine is taken from hydrogen chloride, molybdenum is taken from sodium molybdate, and zinc is taken from zinc sulfate. Sodium molybdate and zinc sulfate are added to sulfuric acid-copper sulfate electrolyte in the form of aqueous solution. The copper ion concentration in the sulfuric acid-copper sulfate electrolyte is 90g / L and the sulfuric acid concentration is 110g / L.

[0054] The preparation method of the electrolytic copper foil of this comparative example is as follows: the above electrolyte is fed into a foil machine, the electrolysis temperature is controlled to be 55°C, the current density is 60A / dm 2 The raw foil is then chromated at a concentration of 25 g / L potassium dichromate, a temperature of 30 °C, and a current density of 6 A / dm 2 The electroplating time is 7 seconds, and the electrolytic copper foil with a foil thickness of 6μm is produced.

[0055] Comparative Example 2

[0056] The electrolyte of this comparative example contains, per liter of sulfuric acid-copper sulfate electrolyte: 17 mg of sodium polydisulfide dipropane sulfonate, 22 mg of chlorine, 12 mg of methylene blue, 150 mg of molybdenum and 300 mg of zinc;

[0057] Wherein, chlorine is taken from hydrogen chloride, molybdenum is taken from sodium molybdate, and zinc is taken from zinc sulfate. Sodium molybdate and zinc sulfate are added to sulfuric acid-copper sulfate electrolyte in the form of aqueous solution. The copper ion concentration in the sulfuric acid-copper sulfate electrolyte is 90g / L and the sulfuric acid concentration is 110g / L.

[0058] The preparation method of the electrolytic copper foil of this comparative example is as follows: the above electrolyte is fed into a foil machine, the electrolysis temperature is controlled to be 55°C, the current density is 60A / dm 2 The raw foil is then chromated at a concentration of 25 g / L potassium dichromate, a temperature of 30 °C, and a current density of 6 A / dm 2 The electrolytic copper foil with a thickness of 6 μm was produced.

[0059] Comparative Example 3

[0060] The electrolyte of this comparative example contains, per liter of sulfuric acid-copper sulfate electrolyte: 17 mg of sodium polydisulfide dipropane sulfonate, 22 mg of chlorine, 12 mg of methylene blue, and 30 mg of octylphenol polyglycol ether;

[0061] Among them, chlorine is taken from hydrogen chloride, the copper ion concentration in sulfuric acid-copper sulfate electrolyte is 90g / L, and the sulfuric acid concentration is 110g / L;

[0062] The preparation method of the electrolytic copper foil of this comparative example is as follows: the above electrolyte is fed into a foil machine, the electrolysis temperature is controlled to be 55°C, the current density is 60A / dm 2 The raw foil is then chromated at a concentration of 25 g / L potassium dichromate, a temperature of 30 °C, and a current density of 6 A / dm 2 The electroplating time is 7 seconds, and the electrolytic copper foil with a foil thickness of 6μm is produced.

[0063] Comparative Example 4

[0064] The electrolyte of this comparative example contains, per liter of sulfuric acid-copper sulfate electrolyte: 17 mg of sodium polydisulfide dipropane sulfonate, 22 mg of chlorine, 12 mg of methylene blue, 30 mg of octylphenol polyglycol ether and 300 mg of zinc;

[0065] The chlorine is taken from hydrogen chloride, and the zinc is taken from zinc sulfate. The zinc sulfate is added to a sulfuric acid-copper sulfate electrolyte in the form of an aqueous solution. The copper ion concentration in the sulfuric acid-copper sulfate electrolyte is 90 g / L and the sulfuric acid concentration is 110 g / L.

[0066] The preparation method of the electrolytic copper foil of this comparative example is as follows: the above electrolyte is fed into a foil machine, the electrolysis temperature is controlled to be 55°C, the current density is 60A / dm 2 The raw foil is then chromated at a concentration of 25 g / L potassium dichromate, a temperature of 30 °C, and a current density of 6 A / dm 2 The electroplating time is 7 seconds, and the electrolytic copper foil with a foil thickness of 6μm is produced.

[0067] Comparative Example 5

[0068] The electrolyte of this comparative example contains, per liter of sulfuric acid-copper sulfate electrolyte: 17 mg of sodium polydisulfide dipropane sulfonate, 22 mg of chlorine, 12 mg of methylene blue, 30 mg of octylphenol polyglycol ether and 150 mg of molybdenum;

[0069] Wherein, chlorine is taken from hydrogen chloride, molybdenum is taken from sodium molybdate, and sodium molybdate is added to sulfuric acid-copper sulfate electrolyte in the form of aqueous solution, the copper ion concentration in the sulfuric acid-copper sulfate electrolyte is 90g / L, and the sulfuric acid concentration is 110g / L;

[0070] The preparation method of the electrolytic copper foil of this comparative example is as follows: the above electrolyte is fed into a foil machine, the electrolysis temperature is controlled to be 55°C, the current density is 60A / dm 2 The raw foil is then chromated at a concentration of 25 g / L potassium dichromate, a temperature of 30 °C, and a current density of 6 A / dm 2 The electroplating time is 7 seconds, and the electrolytic copper foil with a foil thickness of 6μm is produced.

[0071] Comparative Example 6

[0072] The electrolyte of this comparative example contains, per liter of sulfuric acid-copper sulfate electrolyte: 50 mg of sodium polydisulfide dipropane sulfonate, 5 mg of chlorine, 35 mg of methylene blue, 60 mg of octylphenol polyglycol ether, 350 mg of molybdenum, and 20 mg of zinc;

[0073] Wherein, chlorine is taken from hydrogen chloride, molybdenum is taken from sodium molybdate, and zinc is taken from zinc sulfate. Sodium molybdate and zinc sulfate are added to sulfuric acid-copper sulfate electrolyte in the form of aqueous solution. The copper ion concentration in the sulfuric acid-copper sulfate electrolyte is 90g / L, and the sulfuric acid concentration is 110g / L.

[0074] The preparation method of the electrolytic copper foil of this comparative example is as follows: the above electrolyte is fed into a foil machine, the electrolysis temperature is controlled to be 55°C, the current density is 60A / dm 2 The raw foil is then chromated at a concentration of 25 g / L potassium dichromate, a temperature of 30 °C, and a current density of 6 A / dm 2 The electroplating time is 7 seconds, and the electrolytic copper foil with a foil thickness of 6μm is produced.

[0075] During the preparation process of the electrolytic copper foils of the embodiments and comparative examples, the line speed of the foil machine was controlled to prepare electrolytic copper foils of different thicknesses. The results show that the electrolyte provided by the present invention is suitable for the preparation of copper foils of various thicknesses.

[0076] test

[0077] The electrolytic copper foils obtained in Examples 1-5 and Comparative Examples 1-6 were tested for thickness, tensile strength, elongation and breaking energy after heating at 200° C.×10 min.

[0078] The test methods for the above performances are as follows:

[0079] 1. Thickness: For each electrolytic copper foil, the thickness is tested using a mm615 thickness gauge based on IPC-TM-650;

[0080] 2. Tensile strength: For each electrolytic copper foil, the tensile strength was tested using a tensile testing machine manufactured by SHIMADZU based on IPC-TM-650;

[0081] 3. Elongation: For each electrolytic copper foil, the elongation was tested using a tensile testing machine manufactured by SHIMADZU based on IPC-TM-650;

[0082] 4. Fracture energy test: measured according to the test method of ASTM D4830 (Standard test method for characterizing the properties of thermoplastic fabrics for roofing and waterproofing). The test equipment adopts a universal testing machine. For example, the sample is fixed between a clamping plate with a hole with an inner diameter of 44.45 mm and a steel rod with a diameter (probe diameter) of 7.9 mm, a height of 127 mm, and a rod end radius of 3.97 mm. The sample is penetrated at a speed of 300 mm / min to measure the maximum load (fracture energy: N). The test environment is a temperature of 23±2°C and a humidity of 45±5%. Each sample is measured 5 times and the average value is taken.

[0083] The test results are shown in Table 1.

[0084] Table 1 Performance test results of electrolytic copper foil obtained in Examples and Comparative Examples

[0085]

[0086]

[0087] As can be seen from Table 1, the tensile strength of the electrolytic copper foils prepared in Examples 1-5 and Comparative Examples 1-6 is not much different under normal conditions, but the elongation of the electrolytic copper foils obtained in the examples is significantly greater than that of the comparative examples; in addition, the ratio of the breaking energy to the thickness of the electrolytic copper foils prepared in Examples 1-5 is above 1.0N / μm before or after the heat treatment, while the ratio of the breaking energy to the thickness of the electrolytic copper foils prepared in the comparative examples is below 1.0N / μm. Therefore, the electrolytic copper foil prepared by the present invention can effectively improve the breaking energy of the copper foil, and when using the electrolytic copper foil, the copper foil can be prevented from breaking during the manufacturing process of the electrode for the secondary battery or the secondary battery.

[0088] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. An additive for electrolytic copper foil, characterized in that: Contains the following ingredients: Sodium polydisulfide bispropane sulfonate, chlorine, methylene blue, octylphenol polyglycol ether, molybdenum, zinc.

2. The additive for electrolytic copper foil according to claim 1, characterized in that: The octylphenol polyglycol ether has the following structural formula: Among them, n=10-22.

3. The additive for electrolytic copper foil according to claim 1 or 2, characterized in that: The chlorine is obtained from chloride, the molybdenum is obtained from molybdate, and the zinc is obtained from zinc sulfate.

4. The additive for electrolytic copper foil according to claim 3, characterized in that: The chloride is selected from any one of hydrogen chloride, potassium chloride and ammonium chloride; the molybdate is selected from any one of sodium molybdate, potassium molybdate and ammonium molybdate.

5. An electrolyte for electrolytic copper foil using the additive for electrolytic copper foil according to any one of claims 1 to 4, characterized in that: Each liter of electrolyte contains: 5-30 mg of sodium polydisulfide propane sulfonate, 10-40 mg of chlorine, 4-20 mg of methylene blue, 10-50 mg of octylphenol polyglycol ether, 10-300 mg of molybdenum, and 50-800 mg of zinc.

6. The electrolyte for electrolytic copper foil according to claim 5, characterized in that: Each liter of electrolyte contains: 10-25 mg of sodium polydisulfide propane sulfonate, 15-30 mg of chlorine, 6-18 mg of methylene blue, 20-40 mg of octylphenol polyglycol ether, 20-250 mg of molybdenum, and 40-700 mg of zinc.

7. The electrolyte for electrolytic copper foil according to claim 6, characterized in that: Each liter of electrolyte contains: 12-22 mg of sodium polydisulfide propane sulfonate, 18-25 mg of chlorine, 8-15 mg of methylene blue, 25-35 mg of octylphenol polyglycol ether, 100-200 mg of molybdenum, and 200-400 mg of zinc.

8. The electrolyte for electrolytic copper foil according to any one of claims 5 to 7, characterized in that: The electrolyte is a sulfuric acid-copper sulfate electrolyte, and the molybdate and zinc sulfate are both added to the sulfuric acid-copper sulfate electrolyte in the form of aqueous solutions.

9. The electrolyte for electrolytic copper foil according to claim 8, characterized in that: The copper ion concentration in the sulfuric acid-copper sulfate electrolyte is 85-120 g / L, and the sulfuric acid concentration is 90-120 g / L.

10. A method for preparing electrolytic copper foil using the electrolytic solution for electrolytic copper foil according to any one of claims 5 to 9, characterized in that: The following steps are involved: (1) The electrolyte is fed into a foil machine to produce raw foil, and the electrolysis temperature is controlled to be 50-60°C and the current density is 50-70A / dm 2 ; (2) Chromate treatment of raw foil, potassium dichromate concentration of 20-30g / L, temperature of 20-40℃, current density of 5-8A / dm 2 , the plating time is 6-8 seconds.