Method for growing inch-grade all-inorganic CsPbBr3 single crystal by VGF (Vertical Growth Factor) method

Through the four-temperature zone VGF method and multiple impurity disposal treatments, the size and quality problems in the growth of CsPbBr3 single crystals are solved, and large-size and high-quality CsPbBr3 single crystals are achieved to meet the industrial needs of high-energy ray detectors.

CN118910730AActive Publication Date: 2024-11-08DAQING NORMAL UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411265687.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-10
Publication Date
2024-11-08
Estimated Expiration
2044-09-10

AI Technical Summary

Technical Problem

The prior art is difficult to grow large-sized and high-quality CsPbBr3 single crystals, and the crystals grown by the melt method are prone to cracking and have many defects, which cannot meet the industrial needs of high-energy ray detectors.

Method used

The four-temperature zone VGF method is used to grow inch-grade all-inorganic CsPbBr3 single crystals. Through multi-stage heating and gradient cooling control, multiple impurity removal and ultrasonic cleaning treatments are combined to ensure the uniformity of the crystal and the low defects.

Benefits of technology

It realizes high-quality CsPbBr3 single crystal preparation with large size, no cracks, high light transmittance and low defect density, which reduces the preparation cost and improves the success rate of single crystals, and is suitable for commercial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910730A_ABST
    Figure CN118910730A_ABST
Patent Text Reader

Abstract

The invention provides a method for growing an inch-level all-inorganic CsPbBr3 single crystal by a VGF (Vertical Growth Factor) method, and belongs to the technical field of crystal growth. The invention provides a preparation method of an inch-level all-inorganic perovskite single crystal. The preparation method comprises the following steps: firstly, taking CsPbBr3 polycrystal, and carrying out impurity removal pretreatment to obtain a polycrystal precursor; putting the polycrystalline precursor into an ampoule bottle, heating to 100-300 DEG C under the condition that the vacuum degree is 10 <-5 >-10 <-2 > Pa, keeping the temperature for 1-8 hours, and sealing the top end of the ampoule bottle; and heating the ampoule bottle in a segmented manner, preserving heat, fully melting the polycrystalline precursor, and carrying out gradient cooling to room temperature after the heat preservation is finished, so as to obtain the inch-level all-inorganic CsPbBr3 single crystal. The VGF method is adopted, the used VGF furnace is good in heat preservation effect, the internal temperature gradient is uniform, the uniformity of the crystals can be better improved, meanwhile, cracks can be prevented from occurring in the crystals, and preparation of large-size single crystals is facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of crystal growth, and specifically relates to a method for growing inch-scale all-inorganic CsPbBr by VGF method. 3 Single crystal method. Background Art

[0002] With the development of optoelectronic information technology, the application scope of high-energy ray detection has gradually expanded and the application demand has increased day by day. Semiconductor detection materials represented by silicon and germanium are gradually unable to meet the needs of technological development. As the core material of high-energy ray detectors, semiconductor single crystals must have a larger size and higher crystal quality. In response to the development requirements of high-energy ray detectors, detection materials need to meet several characteristics at the same time: ① high average atomic number; ② high resistivity; ③ appropriate bandgap width; ④ large carrier mobility lifetime product, as shown in Table 1.

[0003] Table 1 Requirements for semiconductor materials

[0004]

[0005] Recent studies have shown that CsPbBr 3 Single crystals have many unique properties, such as large light absorption coefficient, large atomic number, high resistivity, large and balanced migration lifetime product, and appropriate bandgap width. These characteristics determine the CsPbBr 3 It is a new generation of ideal material for preparing high-energy ray detectors.

[0006] Currently grown CsPbBr 3 Single crystals mainly include solution method and melt method. However, CsPbBr 3 Single crystal growth still faces many difficulties and challenges, such as small crystal size, easy cracking of crystals, and low crystal transmittance:

[0007] 1) The solution method is to convert PbBr 2 The CsBr powder is dissolved in a solvent in a certain proportion, and the solubility is reduced by changing the temperature, etc., so that crystals are precipitated to achieve the effect of growing single crystals. However, it is difficult to obtain large-size single crystals by solution growth, so it cannot meet the industrial needs of high-energy ray detectors.

[0008] 2) The melt method is mainly divided into the VB method, the VGF method, etc. This method synthesizes a single crystal by heating the polycrystalline precursor to above the melting point to melt the crystal, and then cooling it down to allow the crystal to recrystallize.

[0009] ① The VB method has a constant temperature field, but since the growth process of the VB method is completed by the movement of the crystal itself, this inevitably brings about mechanical vibration, resulting in irregular fluctuations in the crystal growth interface, thereby causing defects in the crystal and reducing the crystal quality.

[0010] ② The VGF method is a type of melt method. Compared with the VB furnace, the VGF furnace has better heat preservation. In addition, this method fixes the crystal and relies on the change of the temperature gradient in the furnace to complete the crystal growth. At present, there is no VGF method for growing all-inorganic inch-level CsPbBr 3 Single crystal reports.

[0011] Compared with single crystal silicon (Si), high purity germanium (HPGe) and other semiconductors commonly used for high energy radiation detection, CsPbBr 3 With lower melting and freezing points, CsPbBr 3 The melt method is more suitable. At present, the diameter of crystals grown by various research groups at home and abroad using the melt method is basically about 10mm, and the maximum is 30mm, and all of them are based on 5N PbBr 2 The single crystal preparation cost of each research group is high and is still in the laboratory research and development stage. In addition, the size of the prepared crystals is basically difficult to meet the industrial development needs of high-energy ray detectors. Therefore, it is of great significance to obtain high-quality single crystals with high transmittance, no cracks, and low defect density. Summary of the invention

[0012] In view of this, the present invention aims to provide a method for growing inch-scale all-inorganic CsPbBr 3 The method for preparing single crystals of perovskite has low growth cost, simple method, easy control, large size of synthesized crystals, uniform distribution of components, and no cracks, which is more suitable for high-quality and large-size CsPbBr 3 Commercial production of single crystals.

[0013] In order to achieve the above objectives, in the first aspect, the present invention provides a method for growing an inch-scale all-inorganic CsPbBr 3 The method of producing a single crystal comprises the following steps:

[0014] Step 1) Take CsPbBr 3 The polycrystal is subjected to a pretreatment for removing impurities to obtain a polycrystal precursor;

[0015] Step 2) The pretreated polycrystalline precursor is placed in a quartz ampoule, and after vacuuming, heating, and sealing, the ampoule is placed in a crystal growth chamber, 4 to 6 temperature measuring thermocouples are inserted and fixed at specific positions, and then the top is covered with an insulation cover;

[0016] Step 3) The crystal growth chamber is heated in sections and then kept warm to fully melt the polycrystalline precursor, and after the insulation is completed, the temperature is gradually lowered to room temperature to obtain an inch-level all-inorganic CsPbBr 3 Single crystal;

[0017] The crystal growth chamber in step 3) is a four-temperature zone VGF furnace, which, from bottom to top, are the first heating zone, the second heating zone, the third heating zone, and the fourth heating zone;

[0018] The segmented heating in step 3) is divided into three stages: the first stage lasts 2 to 6 hours, and the four heating zones are simultaneously heated from room temperature to 300 to 350°C; the second stage lasts 1 to 3 hours, and the first heating zone is heated to 300 to 400°C, the second heating zone is heated to 400 to 500°C, the third heating zone is heated to 500 to 600°C, and the fourth heating zone is heated to 500 to 600°C; the third stage lasts 1 to 3 hours, and the first heating zone is heated to 450 to 550°C, the second heating zone is heated to 500 to 600°C, and the third heating zone is heated to 600 to 650°C, and the temperature of the VGF furnace is increased from bottom to top with a temperature gradient of 2 to 10°C / cm;

[0019] The insulation time in step 3) is 15-30h;

[0020] The gradient cooling in step 3) is divided into three stages: the first stage lasts 20 to 50 hours, and the entire VGF furnace is cooled from the third stage heating temperature to 150 to 180°C, wherein the cooling rate of the third and fourth heating zones is greater than that of the first and second heating zones, thereby reducing the temperature gradient in the VGF furnace; the second stage lasts 10 to 50 hours, and each heating zone is cooled to 60 to 70°C at the same time; the third stage lasts 4 to 8 hours, and each heating zone is cooled to room temperature at the same time.

[0021] Preferably, in step 1), CsPbBr 3 Polycrystalline uses PbBr with a purity of 2N 2 and CsBr powder as raw materials; Preparation of CsPbBr 3 After polycrystalline, CsPbBr 3 Polycrystalline is de impurized 2 to 4 times depending on the impurity content.

[0022] Preferably, the CsPbBr 3 The specific preparation steps of polycrystalline are: take PbBr 2 The CsBr powders were placed in two crucibles, heated to 180-260°C and vacuumed for 10 -5 ~10 -2 Pa and dry for 1 to 3 hours;

[0023] Weigh the dried PbBr in a molar ratio of 1:1 2 and CsBr powder in a mortar and grind thoroughly for 1 to 2 hours until the white PbBr 2 Mixed powder with CsBr and ground into orange-yellow CsPbBr 3After the powder is formed, it is placed in an ampoule, evacuated, heated, and sealed; the ampoule is placed in a VGF furnace, heated to 580-640°C within 3-6 hours and maintained for 15-30 hours; finally, the ampoule is cooled to room temperature within 40-60 hours, and CsPbBr is taken out 3 Polycrystalline.

[0024] Preferably, the CsPbBr 3 The specific steps of polycrystalline impurity removal are: 3 The polycrystalline surface and tail end are treated to remove impurities; then placed in a clean room fume hood for drying; the treated CsPbBr 3 The polycrystal is placed in an ampoule, vacuumed, heated, and sealed; the ampoule is placed in a crystal growth chamber, 4 to 6 temperature measuring thermocouples are inserted and fixed at specific positions, and the top is covered with a heat-insulating cover; the furnace body is heated to 560 to 620° C. within 6 to 10 hours and maintained for 10 to 20 hours; the ampoule is cooled to room temperature within 40 to 100 hours, and the purified CsPbBr is taken out. 3 Polycrystalline.

[0025] Preferably, the impurity removal pretreatment step in step 1) is: grinding CsPbBr with 500-3000 mesh sandpaper 3 The darker impurities on both ends and the surface of the polycrystal are then placed in anhydrous ethanol and ultrasonically cleaned in an ultrasonic cleaning machine for 1 to 2 hours. Finally, the crystal is placed in a clean room fume hood to evaporate the anhydrous ethanol on the surface.

[0026] Preferably, the inner diameter of the quartz ampoule is 25-65 mm, the wall thickness is 2-4 mm, the tip of the ampoule is set with a cone angle of 15-25°, and the length of the shoulder area is 8-15 mm.

[0027] Preferably, the heating temperature in step 2) is 160-300°C, the time is 2-3h; the vacuum degree is 10 -5 ~10 -2 Pa; the time is 1 to 8 hours; the sealing method is hydrogen-oxygen flame sealing; the heating and vacuuming are carried out simultaneously.

[0028] Preferably, the experimental equipment needs to be cleaned before each step. The specific steps are: first rinse with ultrapure water to remove large impurities, soak the rinsed equipment in a mixed solution of hydrochloric acid and sulfuric acid for 10 to 30 minutes, and finally rinse the equipment with ultrapure water and methanol in turn to remove the residual mixed solution of hydrochloric acid and sulfuric acid.

[0029] Preferably, except for cleaning of experimental equipment, furnace loading and crystal processing, the remaining steps need to be carried out in a clean room with a cleanliness level of less than 10ppm.

[0030] The beneficial effects of the present invention include at least:

[0031] 1. The present invention adopts the VGF method. The VGF furnace used has good thermal insulation effect and uniform internal temperature gradient, which is more conducive to improving the uniformity of the crystal. At the same time, it can prevent cracks from appearing inside the crystal, which is conducive to the preparation of large-size single crystals.

[0032] 2. The VGF furnace mentioned in the present invention has stable temperature control and adopts multi-point temperature measurement by thermocouples, which can detect the temperature of various parts of the crystal at any time, and adjust the single crystal growth temperature control parameters in time according to temperature feedback, so as to greatly improve the success rate of single crystal preparation.

[0033] 3. The present invention uses 2N high-quality CsPbBr after treatment 3 Polycrystals are used as precursors, the experimental cost is low, the experimental loss is small, and the equipment is simple, which reduces the cost of single crystal preparation. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 It is the structural schematic diagram of VGF furnace;

[0035] Figure 2 CsPbBr grown in Example 1 3 Schematic diagram of a single crystal;

[0036] Figure 3 This is the XRD pattern of the crystal grown in Example 1;

[0037] Figure 4 This is the transmission spectrum of the crystal grown in Example 1;

[0038] Figure 5 CsPbBr grown in Example 2 3 Schematic diagram of a single crystal;

[0039] Figure 6 CsPbBr grown in Example 3 3 Schematic diagram of the crystal;

[0040] Figure 7 CsPbBr grown in Comparative Example 1 3 Schematic diagram of the crystal;

[0041] Figure 8 CsPbBr grown in Comparative Example 2 3 Schematic diagram of the crystal;

[0042] Fig. 9 CsPbBr grown in Comparative Example 3 3 Schematic diagram of the crystal.

[0043] Wherein: 1. First heating zone; 2. Second heating zone; 3. Third heating zone; 4. Fourth heating zone; 5. Temperature measuring thermocouple Tc 1 ; 6. Temperature measuring thermocouple Tc2 ; 7. Temperature measuring thermocouple Tc 3 ;8. Temperature measuring thermocouple Tc 4 ; 9. Insulation cover; 10. Support tube; 11. CsPbBr 3 Single crystal. DETAILED DESCRIPTION

[0044] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0045] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0046] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0047] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present application description and examples are exemplary only.

[0048] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0049] The "room temperature" and "normal temperature" mentioned in the present invention are all calculated as 25±2°C unless otherwise specified.

[0050] Using a four-zone VGF furnace to produce large-scale CsPbBr 3 The preparation of single crystal, from bottom to top, is the first heating zone, the second heating zone, the third heating zone, and the fourth heating zone. Its structure is as follows Figure 1As shown; the crystal growth crucible is a transparent quartz ampoule with an inner diameter of 2 inches and a wall thickness of 3mm. The tip of the ampoule is set at a cone angle of 15 to 25 degrees, and the length of the shoulder area is 8 to 15mm, wherein the upper end of the shoulder area is connected to the cylindrical equal diameter area as a whole, and the cylindrical equal diameter area can be connected to a molecular pump. The quartz ampoule is sealed by a hydrogen-oxygen flame after evacuation; the experimental cleaning steps are unified as follows: rinse the equipment used for single crystal preparation with ultrapure water, soak the rinsed equipment in a mixed solution of hydrochloric acid and sulfuric acid for 10 to 30 minutes, and finally rinse the residual hydrochloric acid and sulfuric acid mixed solution on the surface of the equipment with ultrapure water and methanol in turn; the cleaned experimental equipment is placed in a fume hood for drying; the conditions for evacuation, heating, and sealing are: heating to 200 to 300°C, the vacuum degree is 10 -5 ~10 -2 Pa, time is 2 to 3 hours, sealed with hydrogen-oxygen flame; the heating and vacuuming are carried out simultaneously.

[0051] Example 1

[0052] This embodiment provides an inch-level CsPbBr 3 The method for preparing a single crystal comprises the following steps:

[0053] 1) Remove PbBr 2 A total of 630 g of CsBr powder was placed in two crucibles, heated to 180 °C and vacuumed (10 - 2 Pa) and dried for 3 h; a high-precision electronic balance was used to weigh the dried PbBr with a molar ratio of 1:1 2 and CsBr powder totaling 600g; reweigh the completed PbBr 2 Mix with CsBr powder in a mortar and grind thoroughly for 2 hours until white PbBr 2 Mixed powder with CsBr and ground into orange-yellow CsPbBr 3 After the powder is formed, it is placed in an ampoule, evacuated, heated, and sealed; the ampoule is placed in a VGF furnace, heated to 600°C within 6 hours and maintained for 15 hours; finally, the ampoule is cooled to room temperature within 40 hours. The tip of the ampoule is set at a 20° cone angle, and the shoulder area is 12 mm long.

[0054] 2) Take out the CsPbBr obtained in step 1) 3 After polycrystalline, polish CsPbBr with 800 grit sandpaper 3 The polycrystalline surface impurities were then placed in an ultrasonic cleaning machine for 1 hour, and the cleaned CsPbBr 3 The polycrystals were placed in a clean room fume hood for drying; CsPbBr 3The polycrystals are placed in an ampoule, vacuumed, heated, and sealed; the ampoule is placed in a crystal growth chamber, four temperature measuring thermocouples are inserted and fixed at specific positions, and the top is covered with a heat-insulating cover; the furnace body is heated to 560°C within 6 hours and maintained for 10 hours; the ampoule is cooled to room temperature within 50 hours, and the purified CsPbBr is taken out. 3 Polycrystalline, repeat this step 3 times.

[0055] 3) Take out the CsPbBr after impurity removal 3 Polycrystalline, polished with 1000 grit sandpaper CsPbBr 3 The impurities on the surface of the polycrystal are removed, and then the polycrystal is ultrasonically cleaned in an ultrasonic cleaning machine for 1 hour. Finally, the crystal is placed in a clean room fume hood to evaporate the surface anhydrous ethanol, and then used as a precursor for single crystal growth;

[0056] 4) Place the precursor in a transparent quartz ampoule, evacuate, heat, and seal the top of the ampoule with an oxyhydrogen flame. Place the ampoule in the crystal growth chamber, insert and fix four temperature measuring thermocouples at characteristic positions, and then cover the top with an insulation cover;

[0057] 5) The segmented heating is divided into three stages: the first stage lasts 4 hours, and the four heating zones are simultaneously heated from room temperature to 300°C; the second stage lasts 3 hours, and the first heating zone is heated to 320°C, the second heating zone is heated to 420°C, the third heating zone is heated to 500°C, and the fourth heating zone is heated to 500°C; the third stage lasts 1 hour, and the first heating zone is heated to 480°C, the second heating zone is heated to 520°C, and the third heating zone is heated to 610°C. After reaching the target temperature, keep the temperature for 25 hours to fully melt the precursor.

[0058] 6) The gradient cooling of the crystal growth chamber is divided into three stages: the first stage lasts for 25 hours, and the entire VGF furnace is cooled from the third stage heating temperature to 180°C. The cooling rates of the third and fourth heating zones are greater than those of the first and second temperature zones, thereby reducing the temperature gradient in the VGF furnace; the second stage lasts for 30 hours, and the temperature is cooled to 65°C at the same time; the third stage lasts for 6 hours, and the temperature is cooled to room temperature at the same time.

[0059] CsPbBr grown in Example 1 3 Schematic diagram of a single crystal Figure 2 As shown in the figure, it can be seen that the obtained single crystal has high overall uniformity, high transmittance, large size, no cracks, and high tail flatness. In order to determine the composition of the product, we conducted an X-ray diffraction test on the sample prepared in Example 1, as shown in the figure. Figure 3 As shown in the figure, the high intensity diffraction peaks indicate good crystallinity and consistent orientation between the grains; the absence of impurity peaks means that the obtained product is high-quality CsPbBr 3 Single crystal. Figure 4CsPbBr obtained in Example 1 3 The transmittance spectrum of the single crystal in the ultraviolet-visible-near infrared-mid-infrared range shows that the transmittance in the range of 700-2000nm can reach more than 80%. The high transmittance indicates fewer defects and high crystal quality.

[0060] Step 3) of the present invention can effectively clean CsPbBr 3 Impurities on the surface of polycrystalline inhibit heterogeneous nucleation during crystal growth, thereby ensuring high uniformity and crack-free single crystals.

[0061] Example 2

[0062] The preparation method of this embodiment is the same as that of Embodiment 1, with the only difference being that, in step 6), the first stage time is 35 hours, and the entire VGF furnace is cooled from the third stage heating temperature to 150°C, wherein the cooling rates of the third and fourth heating zones are greater than those of the first and second temperature zones, thereby reducing the temperature gradient in the VGF furnace; the second stage time is 50 hours, and the temperature is cooled to 60°C at the same time; the third stage time is 4 hours, and the temperature is cooled to room temperature at the same time.

[0063] Example 2 Grown CsPbBr 3 Schematic diagram of a single crystal Figure 5 As shown in the figure, it can be seen that compared with Example 1, the uniformity and transmittance of the single crystal obtained in Example 2 are similar to those in Example 1. It can be obtained that the cooling rate within the scope of the patent requirements can achieve high-quality, inch-level CsPbBr 3 Preparation.

[0064] Example 3

[0065] This embodiment is the same as the preparation method of embodiment 1, except that the segmented heating in step 5) is as follows: the first stage is 5 hours to raise the temperature of the four heating zones from room temperature to 350°C at the same time; the second stage is 3 hours, the first heating zone is raised to 380°C, the second heating zone is raised to 490°C, the third heating zone is raised to 580°C, and the fourth heating zone is raised to 580°C; the third stage is 1 hour, the first heating zone is raised to 480°C, the second heating zone is raised to 550°C, the third heating zone is raised to 640°C, and the temperature is kept at the target temperature for 25 hours to fully melt the crystal.

[0066] Example 3 Grown CsPbBr 3 Schematic diagram of a single crystal Figure 6 As shown in the figure, it can be seen that compared with Example 1 and Example 2, the uniformity and transmittance of the single crystal obtained in Example 3 are similar to those in Example 1.

[0067] This proves that the heating process within the scope of this patent can achieve high-quality, inch-level CsPbBr3 Preparation.

[0068] Comparative Example 1

[0069] Comparative Example 1 is the same as Example 1 in preparation method, except that the segmented heating in step 5) is as follows: the first stage is 5 hours to raise the temperature of the four heating zones from room temperature to 300°C at the same time; the second stage is 3 hours, the first heating zone is raised to 320°C, the second heating zone is raised to 420°C, the third heating zone is raised to 500°C and the fourth heating zone is raised to 500°C; the third stage is 1 hour, the first heating zone is raised to 480°C, the second heating zone is raised to 520°C, the third heating zone is raised to 680°C and the fourth heating zone is raised to 680°C. After reaching the target temperature, the temperature is kept for 25 hours to fully melt the crystal.

[0070] Comparative Example 1 Grown CsPbBr 3 Crystal schematic diagram Figure 7 As shown in the figure, it can be seen that compared with Example 1, the uniformity of the crystal obtained in Comparative Example 1 is poor, the flatness of the tail end is reduced, and there are a lot of CsPb on the surface of the crystal. 2 Br 5 and Cs 4 PbB 6 .

[0071] This is because, during the crystal growth process, PbBr 2 There are other reactions with CsBr. By comparing the preparation methods of the two examples, it can be concluded that although the high temperature zone is set higher than CsPbBr 3 The melting point of 50-100℃ is conducive to the full melting of the crystal, but the volatilization of components caused by overheating will lead to the deviation of the internal components of the crystal, the increase of impurities, and the occurrence of heterogeneous nucleation during the crystal growth process. This proves that the temperature control process of the crystal is one of the important factors affecting the quality of the crystal.

[0072] Comparative Example 2

[0073] Comparative Example 2 is prepared in the same manner as Example 1, except that step 3) of "grinding CsPbBr with 1000-grit sandpaper" is omitted in Comparative Example 2. 3 The crystals were then placed in an ultrasonic cleaning machine for 1 hour for ultrasonic cleaning, and finally placed in a clean room fume hood to evaporate the anhydrous ethanol on the surface.

[0074] Comparative Example 2 Grown CsPbBr 3 Crystal schematic diagram Figure 8 As shown in the figure, it can be seen that compared with Example 1, the uniformity of the crystals obtained in Comparative Example 2 is relatively poor, the cracks are significantly increased, the tail end is dark in color, and there are more impurities.

[0075] The reason is that the process of ultrasonic cleaning of the precursor not only effectively removes the impurity powder remaining after grinding, but also removes particles such as silicon carbide remaining on the sandpaper after crystal grinding that affect the crystal quality, and slows down heterogeneous nucleation during single crystal growth.

[0076] This proves that: CsPbBr 3 The treatment of polycrystalline impurities is also one of the important factors affecting crystal quality.

[0077] Comparative Example 3

[0078] Comparative Example 3 is the same as Example 1 in preparation method, except that the segmented heating in step 5) is as follows: the first stage time is 5 hours to raise the temperature of the four heating zones from room temperature to 300°C at the same time; the second stage time is 3 hours, the first heating zone is raised to 320°C, the second heating zone is raised to 420°C, the third heating zone is raised to 500°C and the fourth heating zone is raised to 500°C; the third stage time is 1 hour, the first heating zone is raised to 480°C, the second heating zone is raised to 520°C, the third heating zone is raised to 680°C and the fourth heating zone is raised to 680°C. After reaching the target temperature, keep warm for 25 hours to fully melt the crystal; at the same time, step 3) "polishing the obtained CsPbBr with 1000 mesh sandpaper" is cancelled. 3 The crystals were then placed in an ultrasonic cleaning machine for 1 hour for ultrasonic cleaning, and finally placed in a clean room fume hood to evaporate the anhydrous ethanol on the surface.

[0079] Comparative Example 3 Grown CsPbBr 3 Schematic diagram of a single crystal Fig. 9 As shown, compared with Example 1, it can be seen from the crystal picture obtained in Comparative Example 3 that the crystal grown in Comparative Example 1 is dark in color, has many internal impurities, poor uniformity, is obviously polycrystalline, and has many overall cracks.

[0080] It can be concluded that the heterogeneous nucleation phenomenon during crystal growth can be reduced by removing impurities through ultrasonic cleaning and precise temperature control process. This not only ensures the uniformity of crystal growth, but also improves the quality of the final single crystal. The optimization of these two process steps is an indispensable and important link in achieving high-quality single crystal growth.

[0081] From the results of Examples 1, 2, 3 and Comparative Examples 1, 2, 3, it can be concluded that the impurity removal treatment of the polycrystalline precursor and the precise temperature control process in the present invention are both effective in obtaining high-quality CsPbBr 3 The key factor of single crystal.

[0082] The above description is only the preferred embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.

Claims

1. A VGF method for growing inch-scale all-inorganic CsPbBr 3 Single crystal method, It is characterized in that The following steps are involved: Step 1) Take CsPbBr 3 The polycrystal is subjected to a pretreatment for removing impurities to obtain a polycrystal precursor; Step 2) The polycrystalline precursor is placed in a quartz ampoule, and after vacuuming, heating, and sealing, the ampoule is placed in a crystal growth chamber, 4 to 6 temperature measuring thermocouples are inserted and fixed at specific positions, and then the top is covered with an insulation cover; Step 3) The crystal growth chamber is heated in sections and then kept warm to fully melt the polycrystalline precursor, and after the insulation is completed, the temperature is gradually lowered to room temperature to obtain an inch-level all-inorganic CsPbBr 3 Single crystal; The crystal growth chamber in step 3) is a four-temperature zone VGF furnace, which, from bottom to top, are the first heating zone, the second heating zone, the third heating zone, and the fourth heating zone; The segmented heating in step 3) is divided into three stages: the first stage lasts 2 to 6 hours, and the four heating zones are simultaneously heated from room temperature to 300 to 350°C; the second stage lasts 1 to 3 hours, and the first heating zone is heated to 300 to 400°C, the second heating zone is heated to 400 to 500°C, the third heating zone is heated to 500 to 600°C, and the fourth heating zone is heated to 500 to 600°C; the third stage lasts 1 to 3 hours, and the first heating zone is heated to 450 to 550°C, the second heating zone is heated to 500 to 600°C, and the third heating zone is heated to 600 to 650°C, and the temperature of the VGF furnace is increased from bottom to top with a temperature gradient of 2 to 10°C / cm; The insulation time in step 3) is 15-30h; The gradient cooling in step 3) is divided into three stages: the first stage lasts 20 to 50 hours, and the entire VGF furnace is cooled from the third stage heating temperature to 150 to 180°C, wherein the cooling rate of the third and fourth heating zones is greater than that of the first and second heating zones, thereby reducing the temperature gradient in the VGF furnace; the second stage lasts 10 to 50 hours, and each heating zone is cooled to 60 to 70°C at the same time; the third stage lasts 4 to 8 hours, and each heating zone is cooled to room temperature at the same time.

2. The preparation method according to claim 1, It is characterized in that In step 1), CsPbBr 3 Polycrystalline uses PbBr with a purity of 2N 2 and CsBr powder as raw materials; Preparation of CsPbBr 3 After polycrystalline, CsPbBr 3 Polycrystalline is de impurized 2 to 4 times depending on the impurity content.

3. The preparation method according to claim 2, It is characterized in that The CsPbBr 3 The specific preparation steps of polycrystalline are: take PbBr 2 The CsBr powders were placed in two crucibles and heated to 180-260°C while evacuating the crucible for 10 -5 ~10 -2 Pa, drying for 1 to 3 hours; Weigh the dried PbBr in a molar ratio of 1:1 2 and CsBr powder in a mortar and grind thoroughly for 1 to 2 hours until the white PbBr 2 Mixed powder with CsBr and ground into orange-yellow CsPbBr 3 After the powder is formed, it is placed in an ampoule, evacuated, heated, and sealed; the ampoule is placed in a VGF furnace, heated to 580-640°C within 3-6 hours and maintained for 15-30 hours; finally, the ampoule is cooled to room temperature within 40-70 hours, and CsPbBr is taken out 3 Polycrystalline.

4. The method according to claim 2, It is characterized in that The CsPbBr 3 The specific steps of polycrystalline impurity removal are: 3 The polycrystalline surface and tail end are treated to remove impurities; the treated CsPbBr 3 The polycrystal is placed in an ampoule, vacuumed, heated, and sealed; the ampoule is placed in a crystal growth chamber, 4 to 6 temperature measuring thermocouples are inserted and fixed at specific positions, and the top is covered with a heat-insulating cover; the furnace body is heated to 560 to 620° C. within 6 to 10 hours and maintained for 10 to 20 hours; the ampoule is cooled to room temperature within 40 to 100 hours, and the purified CsPbBr is taken out. 3 Polycrystalline.

5. The preparation method according to claim 1, It is characterized in that The impurity removal pretreatment step in step 1) is: grinding CsPbBr with 500-3000 mesh sandpaper 3 The darker impurities on both ends and the surface of the polycrystal are then placed in anhydrous ethanol and ultrasonically cleaned in an ultrasonic cleaning machine for 1 to 2 hours. Finally, the crystal is placed in a clean room fume hood to evaporate the anhydrous ethanol on the surface.

6. The preparation method according to claim 1, It is characterized in that In the step 2), the inner diameter of the quartz ampoule is 25-65 mm, the wall thickness is 2-4 mm, the tip of the ampoule is set with a cone angle of 15-25°, and the length of the shoulder area is 8-15 mm.

7. The preparation method according to claim 1, It is characterized in that The heating temperature in step 2) is 160-300°C for 2-3 hours; the vacuum degree is 10 -5 ~10 -2 Pa; the time is 1 to 8 hours; the sealing method is hydrogen-oxygen flame sealing; the heating and vacuuming are carried out simultaneously.

8. The preparation method according to claim 1, It is characterized in that Before each step, the experimental equipment needs to be cleaned. The specific steps are: first rinse with ultrapure water to remove large impurities, soak the rinsed equipment in a mixed solution of hydrochloric acid and sulfuric acid for 10 to 30 minutes, and finally rinse the residual hydrochloric acid and sulfuric acid mixed solution in the equipment with ultrapure water and methanol in turn.

Citation Information

Patent Citations

  • Preparation method of bromine-lead-cesium single crystals

    CN105483825A

  • Visual directional growth device and growth method for large-size bromine-lead-cesium single crystal

    CN110219046A

  • GaAs single crystal growth process

    CN114540955A

  • Method for preparing polycrystals from indium phosphide fragments

    CN116555911A

  • Large-volume cesium-lead-bromine single crystal prepared by vertical Bridgman method as well as preparation method and application thereof

    CN118407112A