Durable waterproof fabric and preparation method thereof

By combining organic acids with waterproofing agents and crosslinking agents through a supercritical carbon dioxide process, a durable waterproof layer is formed, solving the problems of poor water resistance to washing and chemical catalyst residue in the preparation of existing waterproof fabrics, and achieving durable waterproof performance and wide applicability.

CN118910882APending Publication Date: 2024-11-08NANJING BIOSERICA ERA ANTIMICROBIAL MATERIALS TECHNOLOGY GROUP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411069715.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing methods for preparing waterproof fabrics have problems such as poor waterproofing performance, limited application range, and the presence of residual chemical catalysts.

Method used

Organic acids are added to the fabric raw material or fabric using a supercritical carbon dioxide process, and then the fabric is soaked in a mixed solution of waterproofing agent and crosslinking agent. A strong waterproof layer is formed by high-temperature setting, and this process is repeated multiple times to improve the waterproofing effect.

Benefits of technology

It achieves durable waterproofing, avoids chemical catalyst residue, expands the range of applications, and improves the waterproof performance of the fabric.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910882A_ABST
    Figure CN118910882A_ABST
Patent Text Reader

Abstract

The invention discloses a durable waterproof fabric and a preparation method thereof, and the preparation method comprises the following steps: 1) adding an organic acid to a fabric raw material or a fabric by using a supercritical carbon dioxide process to obtain a modified raw material or a modified fabric; (2) soaking the modified fabric obtained in the step (1) or a fabric prepared from the modified raw materials obtained in the step (1) in a mixed solution of a waterproof agent and a cross-linking agent, and then taking out and shaping at high temperature; and 3) repeating the step 2) for several times to obtain the waterproof fabrics with different waterproof degrees. Compared with the prior art, the invention has the following advantages: 1) the technical means of grey yarn modification is adopted to avoid the limitations that the commercial fabric is large in volume, cannot be randomly cut and is not suitable for sequencing batch processing; and 2) the waterproof fabric obtained by the invention makes up the problems that the waterproof function is not washable, the application range is limited, chemical catalysts are left and the like in other treatment methods.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of durable waterproof fabric detection, and in particular relates to a durable waterproof fabric and a preparation method thereof. Background Art

[0002] As the world's love for outdoor sports and leisure activities increases, the market demand for waterproof fabrics continues to grow. Especially in a major textile production and consumption country like China, the waterproof fabric market has great potential.

[0003] In order to meet the needs of fabrics used in water environments, the current technical solution can only achieve waterproofing through post-finishing on the fabric. Conventional waterproofing methods usually directly soak the fabric in a mixed solution of a waterproofing agent and a cross-linking agent, and then high-temperature setting makes the fabric waterproof, but the washing resistance is very poor. Another waterproofing treatment method is to graft citric acid onto the fabric by chemical grafting, and then prepare waterproof fabrics through silica hydrogel and alkyl siloxane, but there are also two problems: 1) The citric acid grafting process requires a catalyst, which is generally an acid or metal compound, and the residue on the fabric will cause a certain degree of health problems to the human body; 2) Since citric acid is a carboxyl-rich substance, this method is limited to hydroxyl-rich fabric materials (cellulose materials), and other materials cannot be made waterproof by this method. Summary of the invention

[0004] Purpose of the invention: The existing technical solutions can only achieve waterproof function by post-finishing on the fabric. In order to improve the problems of the waterproof function of this waterproof fabric preparation method, such as poor resistance to washing, limited application scope, and residual chemical catalyst, the present invention provides a durable waterproof fabric and a preparation method thereof.

[0005] Technical solution: In order to achieve the above-mentioned invention object, the present invention adopts the following technical solution:

[0006] A method for preparing a durable waterproof fabric comprises the following steps:

[0007] 1) Use supercritical carbon dioxide process to add organic acid to fabric raw materials or fabrics to obtain modified raw materials or modified fabrics;

[0008] 2) taking the modified fabric obtained in step 1), or the fabric made of the modified raw material obtained in step 1), and immersing it in a mixed solution of a waterproofing agent and a cross-linking agent, and then taking it out and subjecting it to high temperature setting;

[0009] 3) Repeat step 2) several times to obtain waterproof fabrics with different waterproof levels.

[0010] As a specific implementation scheme, in step 1), the supercritical carbon dioxide process includes the following steps:

[0011] Place the organic acid and fabric raw materials or fabrics in a supercritical carbon dioxide device, set process parameters, start the device, and perform modification.

[0012] As a specific implementation scheme, in step 1), the process parameters of the supercritical carbon dioxide process are: pressure 5-20MPa, temperature 40-80°C, reaction time 10-120min; the mass ratio of the organic acid to the fabric raw material is 1:90-110, and the mass ratio of the organic acid to the fabric is 1:90-110.

[0013] As a specific implementation scheme, in step 1), the fabric raw material includes natural material, chemically synthesized material or regenerated cellulose material; the organic acid includes aliphatic organic acid and aromatic organic acid.

[0014] As a specific implementation scheme, in step 1), the natural material is selected from cotton, linen, wool or silk; the chemical synthetic material is selected from polyester, nylon or spandex; the regenerated fiber material is selected from viscose, tencel or modal; the aliphatic organic acid is selected from citric acid, malic acid, tartaric acid or succinic acid; the aromatic organic acid is selected from hydroxycinnamic acid, caffeic acid, ferulic acid or sinapic acid.

[0015] As a specific implementation scheme, in step 2), the waterproofing agent and the cross-linking agent are respectively prepared into aqueous solutions at a concentration of 2-5%, mixed and fully stirred to obtain a mixed aqueous solution; the soaking time is 5-10s, and the temperature range of high temperature setting is 150-200°C.

[0016] As a specific implementation scheme, in step 2), the waterproofing agent includes a fluorine-containing waterproofing agent and a fluorine-free waterproofing agent, and its main feature is that it contains multiple carboxyl functional groups; preferably, the waterproofing agent is selected from fluorocarbon compounds or long-chain acrylic resins.

[0017] As a specific implementation scheme, in step 2), the cross-linking agent is mainly characterized by containing a -C=N=O functional group, and can effectively undergo condensation cross-linking reaction with an organic acid and a waterproofing agent; preferably, the cross-linking agent is selected from isocyanate, polyurethane aqueous dispersion or water-soluble aliphatic polyisocyanate emulsion.

[0018] As a specific implementation, in step 3), the step is repeated several times, 2-5 times.

[0019] The invention also provides a durable waterproof fabric, which is prepared by the above preparation method.

[0020] In order to meet the use requirements of fabrics in water environments, the existing technical solutions can only achieve waterproof function by post-finishing the fabrics. This method of preparing waterproof fabrics has problems such as the waterproof function is not resistant to washing, limited application scope, and residual chemical catalysts.

[0021] The present invention utilizes supercritical carbon dioxide, which has both liquid solubility and gaseous diffusivity. The solubility can not only swell the polymer fabric but also dissolve the organic acid substance; the diffusivity can diffuse the organic acid into the gaps between the swollen polymer molecular chains. After the supercritical condition is removed, the polymer molecular chains shrink, the carbon dioxide gasifies and escapes, and the organic acid molecules are embedded in the polymer surface.

[0022] The method provided by the present invention can modify fibers and yarns (filaments) and firmly and evenly embed organic acid molecules into the surface of fibers and yarns (filaments). Each yarn of the woven fabric thus contains abundant carboxyl functional groups, which can undergo sufficient condensation and cross-linking reactions with waterproofing agents and cross-linking agents to form a firm and dense waterproof layer.

[0023] Beneficial effects: Compared with the prior art, the present invention has the following advantages: 1) The technical means of raw yarn modification avoids the limitations of large volume of commercial fabrics, inability to cut at will, and unsuitability for batch processing. 2) The waterproof fabric obtained by the present invention makes up for the problems of other treatment methods such as poor washing resistance, limited application range, and residual chemical catalysts. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 The waterproof layer structure of the polyester waterproof fabric prepared in Example 1. DETAILED DESCRIPTION

[0025] The present invention can be better understood according to the following examples. However, the contents described in the examples are only used to illustrate the present invention, and should not and will not limit the invention described in detail in the claims.

[0026] Example 1

[0027] 1) Adding malic acid to polyester yarn using a supercritical carbon dioxide process, the specific method includes the following: weighing polyester yarn and malic acid according to a mass ratio of 100:1, first pouring the malic acid into the additive tank of the supercritical carbon dioxide equipment, and then putting the polyester yarn into the supercritical carbon dioxide equipment, checking to ensure that the equipment is in a normal state and then starting the equipment, the supercritical carbon dioxide conditions are: pressure 5MPa, temperature 80℃, reaction time 20min;

[0028] 2) Select a water-soluble long-chain acrylic resin as a waterproofing agent and a water-soluble aliphatic polyisocyanate emulsion as a cross-linking agent, prepare aqueous solutions at 2% and 3% respectively, mix and stir thoroughly to form a mixed aqueous solution;

[0029] 3) The modified polyester yarn obtained in step 1) is made into fabric through a weaving process, and then immersed in the mixed aqueous solution obtained in step 2), and taken out after 5 seconds for high-temperature setting, with the setting temperature being 160° C.;

[0030] 4) Repeat step 3) twice to obtain polyester waterproof fabric;

[0031] 5) The waterproof layer structure of the prepared polyester waterproof fabric is as follows Figure 1 As shown, wherein R1 and R2 are long-chain alkyl groups.

[0032] Example 2

[0033] 1) Adding malic acid to polyester yarn using a supercritical carbon dioxide process, the specific method includes the following: weighing polyester yarn and malic acid according to a mass ratio of 100:1, first pouring the malic acid into the additive tank of the supercritical carbon dioxide equipment, and then putting the polyester yarn into the supercritical carbon dioxide equipment, checking to ensure that the equipment is in a normal state and then starting the equipment, the supercritical carbon dioxide conditions are: pressure 5MPa, temperature 80℃, reaction time 20min;

[0034] 2) Select a water-soluble long-chain acrylic resin as a waterproofing agent and an isocyanate monomer as a cross-linking agent, prepare aqueous solutions at 2% and 3% respectively, mix and stir thoroughly to form a mixed aqueous solution;

[0035] 3) The modified polyester yarn obtained in step 1) is made into fabric through a weaving process, and then immersed in the mixed aqueous solution obtained in step 2), and taken out after 5 seconds for high-temperature setting, with the setting temperature being 160° C.;

[0036] 4) Repeat step 3) twice to obtain polyester waterproof fabric.

[0037] Example 3

[0038] 1) Adding malic acid to polyester yarn using a supercritical carbon dioxide process, the specific method includes the following: weighing polyester yarn and malic acid according to a mass ratio of 100:1, first pouring the malic acid into the additive tank of the supercritical carbon dioxide equipment, and then putting the polyester yarn into the supercritical carbon dioxide equipment, checking to ensure that the equipment is in a normal state and then starting the equipment, the supercritical carbon dioxide conditions are: pressure 5MPa, temperature 80℃, reaction time 20min;

[0039] 2) Select a water-soluble long-chain acrylic resin as a waterproofing agent and an isocyanate monomer as a cross-linking agent, prepare aqueous solutions at 2% and 3% respectively, mix and stir thoroughly to form a mixed aqueous solution;

[0040] 3) The modified polyester yarn obtained in step 1) is made into fabric through a weaving process, and then immersed in the mixed aqueous solution obtained in step 2), and taken out after 5 seconds for high-temperature setting, with the setting temperature being 160° C.;

[0041] 4) Repeat step 3) 3 times to obtain the polyester waterproof fabric.

[0042] Example 4

[0043] 1) Using a supercritical carbon dioxide process to add malic acid to a fabric made of polyester yarn, the specific method includes the following: weighing the fabric and malic acid according to a mass ratio of 100:1, first pouring the malic acid into the additive tank of the supercritical carbon dioxide equipment, and then putting the fabric into the supercritical carbon dioxide equipment, checking to ensure that the equipment is in a normal state and then starting the equipment, the supercritical carbon dioxide conditions are: pressure 5MPa, temperature 80℃, reaction time 20min;

[0044] 2) Select a water-soluble long-chain acrylic resin as a waterproofing agent and a water-soluble aliphatic polyisocyanate emulsion as a cross-linking agent, prepare aqueous solutions at 2% and 3% respectively, mix and stir thoroughly to form a mixed aqueous solution;

[0045] 3) Soaking the modified fabric obtained in step 1) in the mixed aqueous solution obtained in step 2), taking it out after 5 seconds and setting it at high temperature, with the setting temperature at 160°C;

[0046] 4) Repeat step 3) twice to obtain polyester waterproof fabric.

[0047] Example 5

[0048] 1) Using a supercritical carbon dioxide process to add malic acid to a fabric made of polyester yarn, the specific method includes the following: weighing the fabric and malic acid according to a mass ratio of 100:1, first pouring the malic acid into the additive tank of the supercritical carbon dioxide equipment, and then putting the fabric into the supercritical carbon dioxide equipment, checking to ensure that the equipment is in a normal state and then starting the equipment, the supercritical carbon dioxide conditions are: pressure 5MPa, temperature 80℃, reaction time 20min;

[0049] 2) Select a water-soluble long-chain acrylic resin as a waterproofing agent and an isocyanate monomer as a cross-linking agent, prepare aqueous solutions at 2% and 3% respectively, mix and stir thoroughly to form a mixed aqueous solution;

[0050] 3) Soaking the modified fabric obtained in step 1) in the mixed aqueous solution obtained in step 2), taking it out after 5 seconds and setting it at high temperature, with the setting temperature at 160°C;

[0051] 4) Repeat step 3) twice to obtain polyester waterproof fabric.

[0052] Example 6

[0053] 1) Using a supercritical carbon dioxide process to add malic acid to a fabric made of polyester yarn, the specific method includes the following: weighing the fabric and malic acid according to a mass ratio of 100:1, first pouring the malic acid into the additive tank of the supercritical carbon dioxide equipment, and then putting the fabric into the supercritical carbon dioxide equipment, checking to ensure that the equipment is in a normal state and then starting the equipment, the supercritical carbon dioxide conditions are: pressure 5MPa, temperature 80℃, reaction time 20min;

[0054] 2) Select a water-soluble long-chain acrylic resin as a waterproofing agent and an isocyanate monomer as a cross-linking agent, prepare aqueous solutions at 2% and 3% respectively, mix and stir thoroughly to form a mixed aqueous solution;

[0055] 3) Soaking the modified fabric obtained in step 1) in the mixed aqueous solution obtained in step 2), taking it out after 5 seconds and setting it at high temperature, with the setting temperature at 160°C;

[0056] 4) Repeat step 3) 3 times to obtain the polyester waterproof fabric.

[0057] Experimental Example Waterproof Performance Evaluation

[0058] According to GB / T 4745-2012 "Testing and evaluating the waterproof performance of textiles - Water-wetting method", the polyester waterproof fabric processed by the present invention is tested, and its waterproof effect is shown in the following table:

[0059] Among them, the fabric woven with unmodified polyester yarn in the comparative example is the polyester yarn directly woven into the fabric without modification and then soaked (that is, the polyester yarn and the fabric are not modified), that is, the treatment method is the same as the above-mentioned Examples 1-3, the only difference is that step 1) using malic acid modification step is not included.

[0060]

[0061] The results show that after the waterproofing treatment of the fabric woven with polyester yarn that has not been modified by supercritical carbon dioxide, its anti-wetting performance is poor after 50 washings, and the anti-wetting performance is not resistant to washing; the fabric woven with polyester yarn modified by supercritical carbon dioxide and the polyester fabric directly modified by supercritical carbon dioxide still have good anti-wetting performance after 50 washings, indicating that supercritical carbon dioxide modification can increase the firmness and density of the waterproof layer.

[0062] It should be noted that although fabrics woven from supercritical carbon dioxide modified polyester yarns and polyester fabrics directly modified by supercritical carbon dioxide have comparable anti-wetting properties, due to the limitations of commercial fabrics such as large volume, inability to be cut at will, and unsuitability for batch processing, "first modifying the polyester yarn with supercritical carbon dioxide and then weaving the fabric for waterproofing" is a better solution.

[0063] The above embodiments are the best implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A method for preparing a durable waterproof fabric, characterized in that: The steps include: 1) Use supercritical carbon dioxide process to add organic acid to fabric raw materials or fabrics to obtain modified raw materials or modified fabrics; 2) taking the modified fabric obtained in step 1), or the fabric made of the modified raw material obtained in step 1), and immersing it in a mixed solution of a waterproofing agent and a cross-linking agent, and then taking it out and subjecting it to high temperature setting; 3) Repeat step 2) several times to obtain waterproof fabrics with different waterproof levels.

2. The method for preparing a durable waterproof fabric according to claim 1, characterized in that: In step 1), the supercritical carbon dioxide process comprises the following steps: placing the organic acid and the fabric raw material or the fabric in a supercritical carbon dioxide device, setting process parameters, starting the device, and performing modification.

3. The method for preparing the durable waterproof fabric according to claim 2, characterized in that: In step 1), the process parameters of the supercritical carbon dioxide process are: pressure 5-20MPa, temperature 40-80°C, reaction time 10-120min; the mass ratio of the organic acid to the fabric raw material is 1:90-110, and the mass ratio of the organic acid to the fabric is 1:90-110.

4. The method for preparing a durable waterproof fabric according to claim 1, characterized in that: In step 1), the fabric material includes natural material, chemically synthesized material or regenerated cellulose material; the organic acid includes aliphatic organic acid and aromatic organic acid.

5. The method for preparing the durable waterproof fabric according to claim 4, characterized in that: In step 1), the natural material is selected from cotton, linen, wool or silk; the chemical synthetic material is selected from polyester, nylon or spandex; the regenerated fiber material is selected from viscose, tencel or modal; the aliphatic organic acid is selected from citric acid, malic acid, tartaric acid or succinic acid; the aromatic organic acid is selected from hydroxycinnamic acid, caffeic acid, ferulic acid or sinapic acid.

6. The method for preparing a durable waterproof fabric according to claim 1, characterized in that: In step 2), the waterproofing agent and the cross-linking agent are respectively prepared into aqueous solutions at a concentration of 2-5%, mixed and fully stirred to obtain a mixed aqueous solution; the soaking time is 5-10s, and the high temperature setting temperature range is 150-200°C.

7. The method for preparing a durable waterproof fabric according to claim 1, characterized in that: In step 2), the waterproofing agent includes a fluorine-containing waterproofing agent and a fluorine-free waterproofing agent, and its main feature is that it contains multiple carboxyl functional groups; preferably, the waterproofing agent is selected from fluorocarbon compounds or long-chain acrylic resins.

8. The method for preparing a durable waterproof fabric according to claim 1, characterized in that: In step 2), the cross-linking agent is mainly characterized by containing a -C=N=O functional group, and can effectively undergo condensation cross-linking reaction with an organic acid and a waterproofing agent; preferably, the cross-linking agent is selected from isocyanate, polyurethane aqueous dispersion or water-soluble aliphatic polyisocyanate emulsion.

9. The method for preparing a durable waterproof fabric according to claim 1, characterized in that: In step 3), the process is repeated several times, 2-5 times.

10. A durable waterproof fabric, characterized in that: The durable waterproof fabric is prepared by the preparation method described in any one of claims 1-9.