High-porosity wet paper-based friction material as well as preparation method and application thereof
By using inorganic pore-making agent to generate small molecule gas during the hot pressing and vulcanization of wet paper-based friction materials, regulating porosity and pore size, the problems of safety hazards, high operation difficulty and high cost in the prior art are solved, and high pores are achieved Preparation of rate materials and improvement of friction and wear performance.
Patent Information
- Application Number
- CN202411070426.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-08-06
AI Technical Summary
In the existing preparation methods for wet paper-based friction materials, the organic chemical foaming agent used has safety risks, is difficult to operate, is costly, and has poor environmental protection performance, making it difficult to effectively control porosity and pore size.
Inorganic pore-making agents such as aluminum sulfate, alum and aluminum hydroxide particles are used to generate small molecule gases through chemical reactions during hot pressing and vulcanization, and the porosity and pore size of wet paper-based friction materials are regulated to achieve high porosity material preparation .
It realizes the preparation of high-porosity wet paper-based friction materials with safe, environmental protection and low cost, improves friction and wear performance, simplifies the production process, and avoids the emission of organic and toxic gases.
Smart Images

Figure HDA0004981619390000011 
Figure HDA0004981619390000012 
Figure HDA0004981619390000021
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of friction materials, and in particular to a high-porosity wet paper-based friction material and a preparation method and application thereof. Background Art
[0002] Wet paper-based friction material is a fiber composite material working in oil medium, with cellulose fiber or synthetic fiber as reinforcing fiber, adding friction performance modifier and filler, etc., formed by papermaking process, impregnated with adhesive resin, and hot-pressed and cured. Compared with wet friction materials such as cork rubber-based friction materials, powder metallurgy friction materials, carbon / carbon-based friction materials, wet paper-based friction materials have the advantages of high dynamic friction coefficient, static / dynamic friction coefficient ratio close to 1, strong torque transmission ability, low friction noise, soft and smooth bonding process, good wear resistance and designable structure shape. It is widely used in transmission and braking devices of various vehicles and engineering machinery, such as wet clutch of automobile automatic transmission, motorcycle clutch and wet brake device of heavy vehicle.
[0003] Friction and wear performance is a key indicator of wet paper-based friction materials, which depends on the proportion of raw materials, manufacturing methods and the morphology of the friction surface. When the type and ratio of raw materials are certain, the friction and wear performance is greatly affected by the overall material structure, especially the porosity of the material. When the porosity of the material is high, the oil on the sliding contact surface is easier to penetrate into the material, and the oil film on the sliding contact surface can be removed more effectively. At the same time, the oil has better fluidity inside the material, the temperature of the material surface is relatively low, and the thermal decay is less, so the friction coefficient is higher.
[0004] Chinese patent CN110965385A discloses a method for preparing a pore structure optimized paper-based friction material, wherein a paper-based friction material preform is immersed in a binder solution formed by a surfactant, a thickener and a physical foaming agent, and then subjected to physical foaming, and then subjected to hot pressing and curing treatment to obtain the paper-based friction material. However, the physical foaming agent used in the patent is flammable and volatile, and the steam forms an explosive mixture after mixing with air, most of which can cause human poisoning and environmental pollution, and has poor safety and is difficult to operate in practice.
[0005] Chinese patent CN114197250A discloses a method for preparing a wet paper-based friction material based on foam molding, which uses a foam molding method to adjust the pore structure of the wet paper-based friction material. A surfactant is added to a water dispersion system of natural fibers, synthetic fibers, fillers, and dispersants for foaming. After the foam slurry is dried, a base paper of the paper-based friction material is obtained; then the base paper is dipped in glue, hot-pressed, and cured to obtain a foam-molded wet paper-based friction material. This patent uses micron-level water-based bubbles (water + surfactant + air) as a dispersion medium, which can increase the bulk and porosity of the base paper and achieve the regulation of the porosity and pore structure of the base paper. However, slurry containing a large number of bubbles will cause difficulties in pulp flow and mesh forming, and the amount and size of bubbles are not easy to control.
[0006] Chinese patent CN112064404A discloses a method for preparing a high-porosity paper-based friction material, which effectively regulates the pore structure of the paper-based friction material by introducing chemical foaming technology in the process of preparing the traditional paper-based friction material, and can significantly improve the average pore size and porosity of the material after the hot pressing process. The organic chemical foaming agent used is one or any combination of N,N'-dinitrosopentamethylenetetramine, N,N'-dimethyl-N,N'-dinitrosoterephthalamide, diazoaminobenzene, azodicarbonamide, azobisisobutyronitrile, azodicarboxylic acid esters, barium azodicarboxylate, benzenesulfonylhydrazide, p-toluenesulfonylhydrazide, 4,4'-oxybisbenzenesulfonylhydrazide, 1,3-benzenedisulfonylhydrazide or 3,3'-disulfonylhydrazide diphenyl sulfone; the foaming aid is one or any combination of urea, diethylene glycol, stearic acid, lauric acid, salicylic acid, zinc stearate, glycerol or sorbitol. However, most of the above-mentioned organic chemical foaming agents are toxic and carcinogenic, and some have very strict requirements for storage and use. For example, N,N'-dinitrosopentamethylenetetramine is on the list of Category 3 carcinogens published by the World Health Organization's International Agency for Research on Cancer, diazoaminobenzene is toxic and polluting, and the pure N,N'-dimethyl-N,N'-dinitrosoterephthalamide is an explosive and is sensitive to impact and friction, posing a safety hazard.
[0007] Chinese patent CN108978346A discloses a method for preparing a foamed phenolic resin glue impregnated paper-based friction material, wherein low molecular weight phenolic resin, polyimide resin, water, anhydrous ethanol, emulsifier, thickener, polyacrylamide, chromium salt and additives are mixed, stirred at a constant temperature, and carbon dioxide gas is continuously introduced during the reaction to obtain a foamed phenolic resin glue; the foamed phenolic resin glue is impregnated with wet paper-based friction material base paper, and the foamed phenolic resin glue impregnated paper-based friction material is obtained after hot pressing. This method requires additional equipment, continuous introduction of carbon dioxide gas, and the distribution of the gas in the material is difficult to effectively control.
[0008] Chinese patent CN107326721A discloses a method for preparing a paper-based friction material with uniform pores. First, alumina, potassium feldspar and the like are mixed and ball-milled, and the obtained ball-milled powder is filled into a mold, and mixed short fibers are obtained by high-temperature melt drawing. Then, aluminum isopropoxide powder is mixed and dispersed with glacial acetic acid solution, and then silica sol is added and mixed with tetraethylammonium hydroxide and the like to obtain a modified mixed solution. The mixed short fibers are then added to the modified mixed solution, dispersed and dried, mixed with bamboo fiber and water, and placed on a paper forming device with a screen after delamination treatment. After drying, the phenolic resin ethanol solution is immersed, and after the immersion is completed, the paper-based friction material with uniform pores is obtained. The high-temperature melt drawing needs to be preheated for 25 to 30 minutes under a nitrogen protective atmosphere at 250 to 300°C, and then heated to 1750 to 1800°C at 15°C / min, and kept melted for 1 to 2 hours. After the insulation and melting are completed, the crucible leak is wired with a glass rod. The paper-based friction material prepared in this patent has the characteristics of high friction coefficient and good controllability of void structure, and is an ideal friction material. However, the preparation steps of the paper-based friction material in this patent are complicated, and the high-temperature melt drawing step requires a special high-temperature resistant device, which has high energy consumption and high production cost. Therefore, it is urgent to provide a preparation method of a high-porosity wet paper-based friction material with high reagent safety, simple steps and low cost. Summary of the invention
[0009] In view of this, the purpose of the present invention is to provide a high-porosity wet paper-based friction material and its preparation method and application. The preparation method provided by the present invention has simple steps, uses an inorganic pore-forming agent, is safe and environmentally friendly, has low energy consumption, and has low production cost.
[0010] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0011] The present invention provides a method for preparing a high-porosity wet paper-based friction material, comprising the following steps:
[0012] mixing natural fibers, synthetic fibers, friction modifier fillers and water to obtain a slurry;
[0013] The slurry is dehydrated, formed and then dried to obtain a wet paper-based friction material base paper;
[0014] The wet paper-based friction material base paper is impregnated in a phenolic resin impregnation solution and then dried to obtain a wet paper-based friction material impregnated paper;
[0015] Hot-pressing and vulcanizing the wet paper-based friction material dipped paper to obtain a high-porosity wet paper-based friction material;
[0016] The slurry or the phenolic resin dipping solution also includes a pore-forming agent;
[0017] The pore-forming agent in the slurry includes a water-soluble pore-forming agent and an inorganic strong base, or an insoluble pore-forming agent; the water-soluble pore-forming agent includes aluminum sulfate, or alum and sulfuric acid; the insoluble pore-forming agent includes aluminum hydroxide particles and / or calcium oxalate powder, and the pH value of the slurry containing the inorganic strong base is 6 to 8;
[0018] The pore-forming agent in the phenolic resin dipping solution includes one or more of aluminum hydroxide particles, alum and calcium oxalate powder.
[0019] Preferably, when the slurry further includes aluminum sulfate and an inorganic strong base, the method for preparing the slurry containing a pore-forming agent comprises the following steps: adding aluminum sulfate to the slurry to a pH value of 0.1 to 5, and then adding an inorganic strong base to adjust the pH value to 6 to 8;
[0020] When the slurry further includes alum, sulfuric acid and an inorganic strong base, the preparation method of the slurry containing a pore-forming agent comprises the following steps: adding alum to the slurry, adding sulfuric acid to adjust the pH value to 0.1-5, and then adding an inorganic strong base to adjust the pH value to 6-8; the mass of alum in the slurry accounts for 0.1-5% of the dry weight of the slurry without adding the insoluble pore-forming agent;
[0021] When the slurry further includes an insoluble pore former, the preparation method of the slurry containing the pore former includes the following steps: adding the insoluble pore former to the slurry; the mass of the insoluble pore former accounts for 0.001-10% of the mass of the slurry without the insoluble pore former.
[0022] Preferably, when the phenolic resin dipping solution further includes a pore-forming agent, the mass of the pore-forming agent accounts for 0.1 to 5% of the dry weight of the phenolic resin; and the particle size of the pore-forming agent is 1 to 1000 nm.
[0023] Preferably, the phenolic resin in the phenolic resin dipping solution includes one or more of unmodified phenolic resin, cashew nut shell oil-modified phenolic resin, melamine-modified phenolic resin, latex-modified phenolic resin and boron-modified phenolic resin;
[0024] The solid content of the phenolic resin dipping solution is 20-50%.
[0025] Preferably, the natural fiber includes one or more of hemp fiber, cotton fiber, bamboo fiber and wood pulp fiber;
[0026] The synthetic fiber includes one or more of aramid fiber, carbon fiber, glass fiber, ceramic fiber and polyimide fiber;
[0027] The friction performance modifier filler includes one or more of diatomaceous earth, silicon dioxide, feldspar, barium sulfate, graphite, aluminum oxide and organic friction powder;
[0028] The mass ratio of the natural fiber to the synthetic fiber is 1:0.1-8;
[0029] The mass ratio of the natural fiber to the friction performance modifier filler is 1:0.1-12;
[0030] The solid content of the slurry is 0.5-3%.
[0031] Preferably, the dipping time is 3 to 20 minutes.
[0032] Preferably, the temperature of the hot pressing vulcanization is 180-230° C., the pressure is 1-30 MPa, and the time is 1-30 min.
[0033] The present invention also provides a high-porosity wet paper-based friction material prepared by the preparation method described in the above technical solution.
[0034] Preferably, the weight of the high-porosity wet paper-based friction material is 100-2000 g / m 2 , thickness is 0.2~5mm.
[0035] The present invention also provides the use of the high-porosity wet paper-based friction material described in the above technical solution in a wet clutch or a wet brake device.
[0036] The invention mixes natural fiber, synthetic fiber, friction performance regulator filler and water, dehydrates and forms the obtained slurry, dries, impregnates and dries, and adds pore-forming agent to the slurry or phenolic resin impregnation liquid, and thermally decomposes during hot pressing vulcanization to obtain porous wet paper-based friction material impregnated paper.
[0037] When a water-soluble pore-forming agent and an inorganic strong base are added to the slurry, the porosity of the wet paper-based friction material is regulated by a multi-step chemical reaction of inorganic substances. Aluminum sulfate and alum are both strong acid and weak base salts. In the presence of an inorganic strong base, a hydrolysis reaction will occur in the aqueous solution, generating aluminum hydroxide colloidal precipitates and H in the fiber surface and system. + The solution is acidic. Alkali solution is added to the slurry system to adjust the pH value to 6-8, which will generate a large amount of aluminum hydroxide precipitation. Aluminum hydroxide is easily decomposed by heat, and aluminum oxide and water are generated during the hot pressing vulcanization process. When water vapor escapes, pores are formed inside the material, which can significantly increase the porosity and pore size of the material. The reaction equation is as follows: 2Al(OH)3=Al2O3+3H2O↑. Moreover, the present invention can control the amount of aluminum hydroxide generated by the reaction through the amount of aluminum sulfate and / or alum and inorganic strong alkali in the slurry, and then control the amount of water vapor generated during hot pressing vulcanization, thereby achieving the regulation of the porosity of the wet paper-based friction material.
[0038] When aluminum hydroxide particles and / or calcium oxalate powder are added to the slurry, or one or more of aluminum hydroxide particles, alum and calcium oxalate powder are added to the phenolic resin dipping solution, the above-mentioned pore-forming agent is easily decomposed by heat. During the hot pressing vulcanization process, aluminum hydroxide generates aluminum oxide and water vapor, and alum is dehydrated to generate anhydrous alum and water vapor; monohydrated calcium oxalate begins to lose water at about 180°C and decomposes into anhydrous calcium oxalate and water vapor, and anhydrous calcium oxalate begins to decompose at about 200°C to generate calcium carbonate and carbon monoxide; when water vapor, carbon monoxide, etc. escape, pores are formed inside the material, which can significantly increase the porosity and pore size of the material. The present invention can control the gas (water vapor and / or carbon monoxide) generated during hot pressing vulcanization by controlling the amount of the above-mentioned pore-forming agent added, thereby realizing the regulation of the porosity of the wet paper-based friction material.
[0039] In the present invention, when the main raw materials and production process remain unchanged, a low-cost inorganic pore-forming agent is added to the slurry or the dipping solution, and a reaction occurs during hot pressing vulcanization to release small molecule gas, thereby increasing the porosity of the wet paper-based friction material, and at the same time, the friction coefficient can be increased, and the friction and wear performance of the wet paper-based friction material can be improved. The pore-forming agent used in the present invention is an inorganic substance, which does not emit organic toxic and harmful gases, is more environmentally friendly, and is cheap and easy to operate compared to organic substances. By adjusting the amount of the pore-forming agent added, different amounts of small molecule gas can be generated during the hot pressing vulcanization process, thereby regulating the porosity and pore size of the wet paper-based friction material, overcoming the defects of the prior art such as being environmentally unfriendly and difficult to operate. When the main raw materials remain unchanged, a high-porosity wet paper-based friction material is obtained by adding a low-cost inorganic substance through a composite chemical reaction, which has low cost, increased porosity, and improved friction and wear performance. Moreover, the preparation method provided by the present invention uses environmentally friendly, easily available raw materials with low prices, a simple and easy-to-operate production process, does not emit organic toxic gases, does not require additional equipment and processes, and has a simple operation process. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 This is a pore size distribution diagram of the wet paper-based friction material prepared in Comparative Example 1;
[0041] Figure 2 This is a pore size distribution diagram of the wet paper-based friction material prepared in Comparative Example 2;
[0042] Figure 3 This is a pore size distribution diagram of the wet paper-based friction material prepared in Example 1;
[0043] Figure 4 This is a pore size distribution diagram of the wet paper-based friction material prepared in Example 2;
[0044] Figure 5 This is a pore size distribution diagram of the wet paper-based friction material prepared in Example 3;
[0045] Figure 6 This is a pore size distribution diagram of the wet paper-based friction material prepared in Example 4;
[0046] Figure 7 This is a pore size distribution diagram of the wet paper-based friction material prepared in Comparative Example 3;
[0047] Figure 8 This is a pore size distribution diagram of the wet paper-based friction material prepared in Example 5;
[0048] Fig. 9 This is the pore size distribution diagram of the wet paper-based friction material prepared in Example 6. DETAILED DESCRIPTION
[0049] The present invention provides a method for preparing a high-porosity wet paper-based friction material, comprising the following steps:
[0050] mixing natural fibers, synthetic fibers, friction modifier fillers and water to obtain a slurry;
[0051] Dehydrating the slurry, forming it, and then drying it to obtain base paper;
[0052] The base paper is impregnated in a phenolic resin impregnation solution and then dried to obtain impregnated paper;
[0053] The impregnated paper is subjected to hot pressing and vulcanization to obtain a high-porosity wet-type paper-based friction material;
[0054] The slurry or the phenolic resin dipping solution also includes a pore-forming agent;
[0055] The pore-forming agent in the slurry includes a water-soluble pore-forming agent and an inorganic strong base, or an insoluble pore-forming agent; the water-soluble pore-forming agent includes aluminum sulfate, or alum and sulfuric acid; the insoluble pore-forming agent includes aluminum hydroxide particles and / or calcium oxalate powder, and the pH value of the slurry containing the inorganic strong base is 6 to 8;
[0056] The pore-forming agent in the phenolic resin dipping solution includes one or more of aluminum hydroxide particles, alum and calcium oxalate powder.
[0057] Unless otherwise specified, the materials and equipment used in the present invention are all commercially available products in the art.
[0058] The invention mixes natural fiber, synthetic fiber, friction performance regulator filler and water to obtain slurry.
[0059] In the present invention, the natural fiber preferably includes one or more of hemp fiber, cotton fiber, bamboo fiber and wood pulp fiber, more preferably cotton fiber or hemp fiber-cotton fiber mixture, and the mass ratio of hemp fiber to cotton fiber in the hemp fiber-cotton fiber mixture is preferably 1:1. In the present invention, the diameter of the natural fiber is preferably 1-50 μm, more preferably 10-40 μm; the length of the natural fiber is preferably 0.2-10 mm, more preferably 0.5-5 mm.
[0060] In the present invention, the synthetic fiber preferably includes one or more of aramid fiber, carbon fiber, glass fiber, ceramic fiber and polyimide fiber. In the present invention, the diameter of the synthetic fiber is preferably 1-30 μm, more preferably 3-20 μm; the length of the synthetic fiber is preferably 0.1-10 mm, more preferably 0.3-5 mm. In the present invention, the synthetic fiber preferably includes an aramid fiber-carbon fiber mixture, and the mass ratio of aramid fiber to carbon fiber in the aramid fiber-carbon fiber mixture is preferably 8-13:7-8, more preferably 1:1 or 13:7.
[0061] In the present invention, the mass ratio of the natural fiber to the synthetic fiber is preferably 1:0.1-8, more preferably 1:1-6, further preferably 1:2-4, and specifically preferably 1:0.1, 1:0.5, 1:1, 1:1.5, 1:2, 1:2.5, 1:3, 1:3.5, 1:4, 1:4.5, 1:5, 1:5.5, 1:6, 1:6.5, 1:7, 1:7.5 or 1:8.
[0062] In the present invention, the friction performance modifier filler preferably includes one or more of diatomite, silica, feldspar, barium sulfate, graphite, alumina and organic friction powder; the feldspar preferably includes one or more of sodium feldspar, calcium feldspar, potassium feldspar and barium feldspar; the organic friction powder preferably includes one or more of rubber powder, cashew nut shell oil friction powder, tire powder and amino ester powder. In the present invention, the friction performance modifier filler is more preferably the first composite friction performance modifier filler or the second composite friction performance modifier filler in terms of mass fraction; the first composite friction performance modifier filler preferably includes a mixture of diatomite, feldspar, graphite, rubber powder and cashew nut shell oil friction powder in a mass ratio of 15:5:6:30:20; the second composite friction performance modifier filler preferably includes a mixture of diatomite, feldspar, alumina, graphite and rubber powder in a mass ratio of 23:10:2:15:10. In the present invention, alumina is dispersed in the material, and part of it may cover the surface of natural fiber and synthetic fiber, which can improve the friction coefficient of the material. In the present invention, the particle size of the friction performance modifier filler is preferably 10 to 800 meshes, more preferably 20 to 350 meshes.
[0063] In the present invention, the mass ratio of the natural fiber to the friction performance regulator filler is preferably 1:0.1-12, more preferably 1:1-10, further preferably 1:2-8, and specifically preferably 1:0.1, 1:0.5, 1:1, 1:1.5, 1:2, 1:2.5, 1:3, 1:3.5, 1:4, 1:4.5, 1:5, 1:5.5, 1:6, 1:6.5, 1:7, 1:7.5, 1:8, 1:8.5, 1:9, 1:9.5, 1:10, 1:10.5, 1:11, 1:11.5 or 1:12.
[0064] In the present invention, when the slurry further includes aluminum sulfate and an inorganic strong base, the preparation method of the slurry containing a pore-forming agent preferably includes the following steps: adding aluminum sulfate to the slurry until the pH value is 0.1 to 5 (preferably), and then adding an inorganic strong base to adjust the pH value to 6 to 8 to obtain a slurry containing a pore-forming agent. In the present invention, the aluminum sulfate is preferably used in the form of an aluminum sulfate aqueous solution, and the concentration of the aluminum sulfate aqueous solution is preferably 0.5 to 25wt%, more preferably 1 to 25wt%, further preferably 5 to 20wt%, and most preferably 10 to 15wt%. In the present invention, after adding aluminum sulfate, the pH value of the system is more preferably 0.5 to 4, more preferably 1 to 3, and specifically preferably 0.1, 0.5, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5 or 5. After adding aluminum sulfate to the slurry, it is preferably further stirred, and the stirring temperature is preferably room temperature, and the stirring time is preferably 5 to 30min, more preferably 10 to 20min. In the present invention, the pH value of the system (i.e., the slurry containing the pore-forming agent) after adding the inorganic strong base is more preferably 6.5-7.5, and more preferably 7. In the present invention, the inorganic strong base is preferably used in the form of an inorganic strong base aqueous solution, and the solid content of the inorganic strong base aqueous solution is preferably 1-30%, more preferably 3-25%, more preferably 5-20%, and most preferably 10-15%; the inorganic strong base preferably includes one or more of sodium hydroxide, potassium hydroxide and barium hydroxide.
[0065] Aluminum sulfate and alum are both strong acid and weak base salts. In the presence of inorganic strong base, hydrolysis reaction will occur in aqueous solution to generate aluminum hydroxide colloidal precipitate and H + , the solution is acidic. Taking aluminum sulfate as an example, the reaction equation is Al 3+ +3H2O=Al(OH)3+3H + When the system pH value is less than 3.0, Al(H2O)6 3+It exists in the form of Al(OH)3; when the pH value is greater than 5.8, it exists entirely in the form of Al(OH)3. When alkali solution is added to the slurry system and the pH value is adjusted to 6-8, a large amount of aluminum hydroxide precipitation will be generated. The reaction equation is Al2(SO4)3+6NaOH=2Al(OH)3↓+3Na2SO4. Aluminum hydroxide is easily decomposed by heat, and aluminum oxide and water are generated during the hot pressing vulcanization process. When water vapor escapes, pores are formed inside the material, which can significantly increase the porosity and pore size of the material. The reaction equation is as follows: 2Al(OH)3=Al2O3+3H2O↑. Moreover, the present invention can control the amount of aluminum hydroxide generated by the reaction through the amount of aluminum sulfate and / or alum and inorganic strong alkali in the slurry, and then control the amount of water vapor generated during hot pressing vulcanization, thereby achieving the regulation of the porosity of the wet paper-based friction material.
[0066] In the present invention, when the slurry further includes alum, sulfuric acid and an inorganic strong base, the preparation method of the slurry containing a pore-forming agent preferably includes the following steps: adding alum to the slurry, adding sulfuric acid to adjust the pH value to 0.1-5, and then adding an inorganic strong base to adjust the pH value to 6-8; the amount of alum in the slurry accounts for 0.1-5% of the dry weight of the slurry without adding the insoluble pore-forming agent. In the present invention, the alum is preferably used in the form of an alum aqueous solution, and the concentration of the alum solution is preferably 0.5-25wt%, more preferably 1-25wt%, further preferably 5-20wt%, and most preferably 10-15wt%. In the present invention, the mass of alum (KAl(SO4)2·12H2O) in the slurry preferably accounts for 0.1-5% of the dry weight of the slurry without adding insoluble pore-forming agent, preferably 0.5-4%, more preferably 1-3%, specifically preferably 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5% or 5%. In the present invention, the pH value after adding sulfuric acid is more preferably 0.5-4, more preferably 1-3, specifically preferably 0.1, 0.5, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5 or 5. In the present invention, after adding alum and sulfuric acid to the slurry, it is preferably further stirred, the stirring temperature is preferably room temperature, and the stirring time is preferably 5-30 minutes, more preferably 10-20 minutes. In the present invention, the pH value of the system (i.e., the slurry containing the pore-forming agent) after adding the inorganic strong base is more preferably 6.5-7.5, and more preferably 7. In the present invention, the inorganic strong base is preferably used in the form of an inorganic strong base aqueous solution, and the solid content of the inorganic strong base aqueous solution is preferably 1-30%, more preferably 3-25%, more preferably 5-20%, and most preferably 10-15%; the inorganic strong base preferably includes one or more of sodium hydroxide, potassium hydroxide and barium hydroxide.
[0067] In the present invention, when the slurry also includes an insoluble pore-forming agent, the preparation method of the slurry containing the pore-forming agent includes the following steps: adding an insoluble pore-forming agent to the slurry to obtain a slurry containing the pore-forming agent; the insoluble pore-forming agent includes one or more of aluminum hydroxide particles, calcium oxalate powder and magnesium hydroxide. In the present invention, the particle size of the insoluble pore-forming agent is preferably 100-800 mesh, more preferably 200-500 mesh; the purity of the aluminum hydroxide particles is preferably chemically pure or analytically pure; the aluminum hydroxide particles are preferably obtained by grinding aluminum hydroxide; the equipment used for grinding preferably includes at least one of a ball mill, a sand mill and a bead mill; the present invention has no special restrictions on the diameter of the grinding beads, the ball-to-material ratio and the grinding time used for the grinding, as long as the aluminum hydroxide particles with a particle size of can be obtained. In the present invention, the mass of the water-insoluble pore-forming agent preferably accounts for 0.001-10% of the mass of the slurry to which the insoluble pore-forming agent is not added, more preferably 0.1-8%, further preferably 1-5%, specifically preferably 0.001%, 0.01%, 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9%, 9.5% or 10%.
[0068] When aluminum hydroxide particles and / or calcium oxalate powder are added to the slurry, or one or more of aluminum hydroxide particles, alum and calcium oxalate powder are added to the phenolic resin dipping solution, the above-mentioned insoluble pore-forming agent is easily decomposed by heat. During the hot pressing vulcanization process, aluminum hydroxide generates aluminum oxide and water vapor, and alum is dehydrated to generate anhydrous alum and water vapor; monohydrated calcium oxalate begins to lose water at about 180°C and decomposes into anhydrous calcium oxalate and water vapor, and anhydrous calcium oxalate begins to decompose at about 200°C to generate calcium carbonate and carbon monoxide; when water vapor, carbon monoxide, etc. escape, pores are formed inside the material, which can significantly increase the porosity and pore size of the material. The present invention can control the gas (water vapor and / or carbon monoxide) generated during hot pressing vulcanization by controlling the amount of the above-mentioned pore-forming agent added, so as to achieve the regulation of the porosity of the wet paper-based friction material.
[0069] The present invention has no special limitation on the mixing, and a mixing method well known to those skilled in the art may be adopted, such as stirring and mixing.
[0070] In the present invention, the solid content of the slurry is preferably 0.5-3%, more preferably 0.5-2.5%, further preferably 1-2, and most preferably 1.5%.
[0071] After obtaining the slurry, the present invention dehydrates the slurry, forms it, and then dries it to obtain base paper.
[0072] In the present invention, the dehydration forming preferably includes: pouring the slurry into a former or a sheet maker, vacuum dehydrating the slurry after it is evenly dispersed to obtain a first wet paper web, and pressing and dehydrating the first wet paper web to obtain a second wet paper web.
[0073] In the present invention, the vacuum degree of the vacuum dehydration is preferably 0.01 to 0.06 MPa, more preferably 0.02 to 0.05 MPa, and further preferably 0.03 to 0.04 MPa; the present invention has no special limitation on the time of the vacuum dehydration, so that the solid content of the first wet paper web is 10 to 25%, and the solid content is more preferably 15 to 20%. The specific time of the vacuum dehydration is 3 to 300 s.
[0074] In the present invention, the squeezing dehydration is preferably performed on a press. In the present invention, the moisture content of the second wet paper web is preferably 25 to 50%, more preferably 30 to 45%, and further preferably 35 to 40%.
[0075] In the present invention, the drying temperature is preferably 70 to 110°C, more preferably 80 to 100°C, and further preferably 90 to 95°C; the drying time is preferably 3 to 600s, more preferably 50 to 500s, and further preferably 100 to 300s; the drying is preferably carried out in a drying cylinder, a vacuum dryer or an oven.
[0076] After the base paper is obtained, the base paper is dipped in a phenolic resin dipping solution and then dried to obtain the dipped paper.
[0077] In the present invention, when the slurry does not contain a pore-forming agent, the phenolic resin dipping solution further comprises a pore-forming agent; the pore-forming agent in the phenolic resin dipping solution comprises one or more of aluminum hydroxide particles, alum and calcium oxalate powder.
[0078] In the present invention, the particle size of the pore-forming agent is preferably 1 to 1000 nm, more preferably 50 to 950 nm, and further preferably 100 to 500 nm; the purity of the aluminum hydroxide particles is preferably chemically pure or analytically pure; the aluminum hydroxide particles are preferably obtained by grinding aluminum hydroxide; the equipment used for the grinding preferably includes at least one of a ball mill, a sand mill, and a bead mill; the present invention has no special restrictions on the diameter of the grinding beads, the ball-to-material ratio, and the grinding time used for the grinding, as long as aluminum hydroxide particles with a particle size of 1 to 1000 nm can be obtained. In the present invention, the mass of the pore-forming agent preferably accounts for 0.1 to 5% of the dry weight of the phenolic resin, more preferably 0.5 to 4.5%, further preferably 1 to 2%, and specifically preferably 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3% 3.5%, 4%, 4.5% or 5%.
[0079] In the present invention, the phenolic resin in the phenolic resin dipping solution preferably includes one or more of unmodified phenolic resin (pure phenolic resin), cashew nut shell oil-modified phenolic resin, melamine-modified phenolic resin, latex-modified phenolic resin and boron-modified phenolic resin; the present invention has no special limitation on the phenolic resin, and it is prepared by a commercially available product well known to those skilled in the art or a preparation method well known to those skilled in the art. In a specific embodiment of the present invention, the phenolic resin is purchased from Shengquan Group. In the present invention, the solvent in the phenolic resin dipping solution preferably includes ethanol. In the present invention, the solid content of the phenolic resin dipping solution is preferably 20-50%, more preferably 25-45%, further preferably 30-40%, and most preferably 35%.
[0080] In the present invention, the solid content of the phenolic resin dipping solution is preferably 20-50%, more preferably 25-45%, further preferably 30-40%, and most preferably 35%; when there is no pore-forming agent in the phenolic resin dipping solution, the solid content is the mass fraction of the dry weight of the phenolic resin; when there is a pore-forming agent, the solid content is the total mass fraction of the dry weight of the phenolic resin and the pore-forming agent.
[0081] In the present invention, when the phenolic resin impregnation solution also contains a pore-forming agent, the phenolic resin impregnation solution is preferably obtained by mixing phenolic resin, aluminum hydroxide particles and ethanol. In the present invention, the mixing temperature is preferably room temperature, the mixing time is preferably 1 to 60 minutes, more preferably 5 to 50 minutes, more preferably 10 to 30 minutes; the mixing method preferably includes stirring mixing and / or ultrasonic mixing, more preferably stirring mixing, or ultrasonic mixing first and then stirring mixing.
[0082] In the present invention, the dipping temperature is preferably room temperature, and the dipping time is preferably 3 to 20 minutes, more preferably 3 to 20 minutes, and further preferably 3 to 20 minutes.
[0083] In the present invention, the glue content of the dipstick is preferably 20-40%, more preferably 30-35%, specifically preferably 30.3%, 30.5%, 32.3% or 32.4%; wherein, glue content = (mass of wet paper-based friction material - mass of base paper) / mass of wet paper-based friction material × 100%.
[0084] After obtaining the impregnated paper, the present invention performs hot pressing vulcanization on the impregnated paper to obtain a high-porosity wet paper-based friction material.
[0085] In the present invention, the temperature of the hot press vulcanization is preferably 180 to 230° C., more preferably 190 to 220° C., and further preferably 200 to 210° C.; the pressure of the hot press vulcanization is preferably 1 to 30 MPa, more preferably 1.5 to 10 MPa, and further preferably 2 to 5 MPa; the time of the hot press vulcanization is preferably 1 to 30 min, more preferably 3 to 20 min, and further preferably 5 to 10 min; the hot press vulcanization is preferably carried out in a vulcanizer.
[0086] The present invention provides a high-porosity wet paper-based friction material prepared by the preparation method described in the above technical solution.
[0087] In the present invention, the weight of the high porosity wet paper-based friction material is preferably 100 to 2000 g / m 2 , more preferably 200 to 1500 g / m 2 , more preferably 300 to 1000 g / m 2 , preferably 341g / m 2 , 345g / m 2 , 366g / m 2 , 398g / m 2 , 400g / m 2 , 401g / m 2 , 409g / m 2 , 410g / m 2; The thickness of the high porosity wet paper-based friction material is preferably 0.2-5 mm, more preferably 0.25-2 mm, further preferably 0.3-1 mm, most preferably 0.35-0.5 mm, specifically preferably 0.379 mm, 0.386 mm, 0.398 mm, 0.400 mm, 0.412 mm, 0.414 mm or 0.416 mm; The porosity of the high wear-resistant wet paper-based friction material is preferably 25.1%, 26.9%, 27%, 29.9%, 44.3%, 46.1% or 46.8%; The average pore size of the high wear-resistant wet paper-based friction material is specifically preferably 2.1721 μm, 2.3524 μm, 2.3325 μm , 3.1700 μm, 3.4131 μm, 3.4178 μm or 4.0456 μm; the dynamic friction coefficient of the highly wear-resistant wet paper-based friction material is preferably ≥0.094, more preferably 0.094-0.121, and specifically preferably 0.094, 0.096, 0.102, 0.108, 0.110, 0.119 or 0.121; the static friction coefficient of the highly wear-resistant wet paper-based friction material is preferably ≥0.108, more preferably 0.108-0.134, and specifically preferably 0.108, 0.110, 0.113, 0.128, 0.130 or 0.134; the wear rate of the highly wear-resistant wet paper-based friction material is preferably ≤4.5×10 -7 cm 2 / J, preferably 2×10 -7 cm 2 / J, 3×10 -7 cm 2 / J, 4×10 -7 cm 2 / J or 4.5×10 -7 cm 2 / J.
[0088] The present invention provides the use of the high-porosity wet paper-based friction material described in the above technical solution in a wet clutch or wet brake device. In the present invention, the high-porosity wet paper-based friction material is preferably used in wet clutches or wet brake devices of various vehicles or engineering machinery, and is more preferably used in wet clutches of automobile automatic transmissions, motorcycle clutches or heavy vehicle wet brake devices; the high-porosity wet paper-based friction material preferably works in an oil medium.
[0089] In order to further illustrate the present invention, a high-porosity wet paper-based friction material provided by the present invention, a preparation method thereof and an application thereof are described in detail below in conjunction with embodiments, but they should not be construed as limiting the scope of protection of the present invention.
[0090] In the following examples and comparative examples, the feldspar is potassium feldspar; the phenolic resin is the phenolic resin used for friction materials of Shengquan Group; and the rubber powder is purchased from Cardolite Corporation.
[0091] Comparative Example 1
[0092] In terms of mass, 8 parts of cotton fiber, 8 parts of aramid fiber, 8 parts of carbon fiber, 15 parts of diatomaceous earth, 5 parts of feldspar, 6 parts of graphite, 30 parts of rubber powder, and 20 parts of cashew nut shell oil friction powder are uniformly dispersed with water to obtain a slurry with a solid content of 1.5%. The slurry is poured into a sheet maker, the slurry is uniformly dispersed, and dehydrated to a solid content of 10-25% under a vacuum degree of 0.01-0.06MPa, and then further dehydrated with a press to obtain a wet paper web with a moisture content of 40%, which is placed in a 95°C vacuum dryer for drying to obtain base paper. The base paper is placed in a phenolic resin ethanol solution with a solid content of 30%, dipped in glue at room temperature for 10 minutes, taken out, and dried at 105°C for 10 minutes to obtain dipped paper with a glue content of 29.7%. The dipped paper is placed on a vulcanizer and hot-pressed and vulcanized for 5 minutes at 200°C and 2MPa to obtain a high-porosity wet paper-based friction material. The weight of high porosity wet paper-based friction material is 408g / m 2 , thickness is 389μm.
[0093] The porosity of the high-porosity wet paper-based friction material measured by a full-automatic true density analyzer is 23.0%, and the average pore size of the material measured by a Capillary Flow Porometer is 3.0078 μm. The pore size distribution is as follows: Figure 1 shown.
[0094] The friction and wear properties of the high-porosity wet paper-based friction material were tested using an MM2000 friction performance tester. Under the conditions of a rotation speed of 2000 r / min and a pressure of 0.4 MPa, the dynamic friction coefficient of the wet paper-based friction material was 0.084 and the static friction coefficient was 0.095. After 2000 tests, the wear rate was 5×10 -7 cm2 / J. Meets the requirements of Class 2 and Class 3 products in the national standard GB / T37208-2018 non-metallic paper-based wet friction materials.
[0095] Comparative Example 2
[0096] In terms of mass, 10 parts of cotton fiber, 10 parts of hemp fiber, 13 parts of aramid fiber, 7 parts of carbon fiber, 23 parts of diatomaceous earth, 10 parts of feldspar, 2 parts of alumina, 15 parts of graphite, and 10 parts of rubber powder are uniformly dispersed with water to obtain a slurry with a solid content of 1.7%. The slurry is poured into a sheet maker, and after the slurry is uniformly dispersed, it is dehydrated to a solid content of 10-25% under a vacuum degree of 0.01-0.06MPa, and then further dehydrated with a press to obtain a wet paper web with a moisture content of 41%, which is placed in a 105°C drying cylinder for drying to obtain base paper. The base paper is placed in a phenolic resin ethanol solution with a solid content of 34%, dipped in glue at room temperature for 15 minutes, taken out, and dried at 100°C for 30 minutes to obtain dipped paper with a glue content of 32.3%. The dipped paper is placed on a vulcanizer and hot-pressed and vulcanized for 3 minutes at 200°C and 4MPa to obtain a high-porosity wet paper-based friction material. The basis weight of high porosity wet paper-based friction material is 338g / m 2 , thickness is 391μm.
[0097] The porosity of the high-porosity wet paper-based friction material was measured by a fully automatic true density analyzer to be 44.1%, and the average pore size of the material was measured by a Capillary Flow Porometer to be 1.9732 μm. The pore size distribution is as follows: Figure 2 shown.
[0098] The friction and wear performance of the high-porosity wet paper-based friction material was tested using an MM2000 friction performance tester. Under the conditions of a speed of 2000r / min and a pressure of 0.4MPa, the dynamic friction coefficient of the wet paper-based friction material was 0.095 and the static friction coefficient was 0.106, meeting the requirements of Class 2 and Class 3 products in the national standard GB / T37208-2018 non-metallic paper-based wet friction materials.
[0099] Example 1
[0100] In terms of mass fraction, 8 parts of cotton fiber, 8 parts of aramid fiber, 8 parts of carbon fiber, 15 parts of diatomaceous earth, 5 parts of feldspar, 6 parts of graphite, 30 parts of rubber powder, and 20 parts of cashew nut shell oil friction powder are uniformly dispersed with water to obtain a slurry with a solid content of 1.5%. The slurry is poured into a sheet maker, and after the slurry is uniformly dispersed, it is vacuum dehydrated to a solid content of 10-25% under a vacuum degree of 0.01-0.06MPa, and then further dehydrated with a press to obtain a wet paper web with a moisture content of 40%, which is placed in a 95°C vacuum dryer for drying to obtain base paper. Chemically pure aluminum hydroxide is ground in a ball mill for 55 minutes, the diameter of the grinding beads is 5-10mm, and the ball-to-material ratio is 15:1 to obtain aluminum hydroxide particles with an average particle size of 930nm. The aluminum hydroxide particles are added to a phenolic resin ethanol solution with a solid content of 30%, and mechanically stirred at room temperature for 20 minutes to obtain a phenolic resin impregnation solution. The base paper was immersed in the above phenolic resin dipping solution at room temperature for 10 minutes, taken out, and dried at 105°C for 10 minutes to obtain the dipped paper with a glue content of 30.1%. The dipped paper was placed on a vulcanizer and hot-pressed and vulcanized at 200°C and 2MPa for 5 minutes to obtain a high-porosity wet paper-based friction material. The quantitative value of the high-porosity wet paper-based friction material is 401g / m 2 The thickness is 400 μm. The mass of aluminum hydroxide particles accounts for 1.5% of the dry weight of the phenolic resin.
[0101] The porosity of the high-porosity wet paper-based friction material measured by a fully automatic true density analyzer is 27.0%, and the average pore size of the material measured by a Capillary Flow Porometer is 3.4178 μm. The pore size distribution is as follows: Figure 3 shown.
[0102] The friction and wear performance of the high-porosity wet paper-based friction material was tested using an MM2000 friction performance tester. Under the conditions of a rotation speed of 2000r / min and a pressure of 0.4MPa, the dynamic friction coefficient of the high-porosity wet paper-based friction material was 0.102, which was 7.4% higher than that of comparative example 1; the static friction coefficient was 0.110, which was 3.8% higher than that of comparative example 1. It meets the requirements of Class 2 and Class 3 products in the national standard GB / T37208-2018 non-metallic paper-based wet friction materials.
[0103] Example 2
[0104] In terms of mass fraction, 8 parts of cotton fiber, 8 parts of aramid fiber, 8 parts of carbon fiber, 15 parts of diatomaceous earth, 5 parts of feldspar, 6 parts of graphite, 30 parts of rubber powder, and 20 parts of cashew nut shell oil friction powder are uniformly dispersed with water to obtain a slurry with a solid content of 1.5%. The slurry is poured into a sheet maker, and after the slurry is uniformly dispersed, it is vacuum dehydrated to a solid content of 10-25% under a vacuum degree of 0.01-0.06MPa, and then further dehydrated with a press to obtain a wet paper web with a moisture content of 40%, which is placed in a 105°C oven for drying to obtain base paper. Chemically pure aluminum hydroxide is ground in a bead mill for 45 minutes, the diameter of the grinding beads is 3-5mm, and the ball-to-material ratio is 20:1 to obtain aluminum hydroxide particles with an average particle size of 200nm. The aluminum hydroxide particles are added to a phenolic resin ethanol solution with a solid content of 29%, and mechanically stirred at room temperature for 30 minutes to obtain a phenolic resin impregnation solution. The base paper was immersed in the above phenolic resin dipping solution at room temperature for 10 minutes, taken out, and dried at 105°C for 20 minutes to obtain dipping paper with a glue content of 29.5%. The dipping paper was placed on a vulcanizer and hot-pressed and vulcanized at 200°C and 2MPa for 5 minutes to obtain a high-porosity wet paper-based friction material. The quantitative value of the high-porosity wet paper-based friction material is 398g / m 2 The thickness is 414 μm. The mass of aluminum hydroxide particles accounts for 2% of the dry weight of the phenolic resin.
[0105] The porosity of the high-porosity wet paper-based friction material was measured to be 29.9% by a fully automatic true density analyzer, and the average pore size of the material was measured to be 4.0456 μm by a Capillary Flow Porometer. The pore size distribution is as follows: Figure 4 shown.
[0106] The friction and wear performance of the high-porosity wet paper-based friction material was tested using an MM2000 friction performance tester. Under the conditions of a rotation speed of 2000r / min and a pressure of 0.4MPa, the dynamic friction coefficient of the high-porosity wet paper-based friction material was 0.110, which was 15.8% higher than that of comparative example 1; the static friction coefficient was 0.128, which was 20.8% higher than that of comparative example 1. It meets the requirements of Class 2 and Class 3 products in the national standard GB / T37208-2018 non-metallic paper-based wet friction materials.
[0107] Example 3
[0108] In terms of mass, 10 parts of cotton fiber, 10 parts of hemp fiber, 13 parts of aramid fiber, 7 parts of carbon fiber, 23 parts of diatomaceous earth, 10 parts of feldspar, 2 parts of alumina, 15 parts of graphite, and 10 parts of rubber powder are uniformly dispersed with water to obtain a slurry with a solid content of 1.9%. The slurry is poured into a sheet maker, and after the slurry is uniformly dispersed, it is vacuum dehydrated to a solid content of 10-25% under a vacuum degree of 0.01-0.06MPa, and then further dehydrated with a press to obtain a wet paper web with a moisture content of 41%, which is placed in a 105°C drying cylinder for drying to obtain base paper. Aluminum hydroxide is ground in a ball mill for 55 minutes, the diameter of the grinding beads is 1-2mm, and the ball-to-material ratio is 20:1 to obtain aluminum hydroxide particles with an average particle size of 100nm. The aluminum hydroxide particles are added to a phenolic resin ethanol solution with a solid content of 30%, and mechanically stirred at room temperature for 30 minutes to obtain a phenolic resin impregnation solution. The base paper was immersed in the above phenolic resin dipping solution at room temperature for 10 minutes, taken out, and dried at 80°C for 40 minutes to obtain the dipped paper with a glue content of 28.9%. The dipped paper was placed on a vulcanizer and hot-pressed and vulcanized at 200°C and 4MPa for 3 minutes to obtain a high-porosity wet paper-based friction material. The quantitative value of the high-porosity wet paper-based friction material is 366g / m 2 , with a thickness of 414 μm. The mass of aluminum hydroxide particles accounts for 1% of the dry weight of the phenolic resin.
[0109] The porosity of the high-porosity wet paper-based friction material was measured by a fully automatic true density analyzer to be 46.1%, and the average pore size of the material was measured by a Capillary Flow Porometer to be 2.1721 μm. The pore size distribution is as follows: Figure 5 shown.
[0110] The friction and wear performance of the high-porosity wet paper-based friction material was tested using an MM2000 friction performance tester. Under the conditions of a rotation speed of 2000r / min and a pressure of 0.4MPa, the dynamic friction coefficient of the high-porosity wet paper-based friction material was 0.119, which was 25.3% higher than that of comparative example 2; the static friction coefficient was 0.134, which was 26.4% higher than that of comparative example 2. It meets the requirements of Class 2 and Class 3 products in the national standard GB / T37208-2018 non-metallic paper-based wet friction materials.
[0111] Example 4
[0112] In terms of mass, 10 parts of cotton fiber, 10 parts of hemp fiber, 13 parts of aramid fiber, 7 parts of carbon fiber, 23 parts of diatomaceous earth, 10 parts of feldspar, 2 parts of alumina, 15 parts of graphite, and 10 parts of rubber powder are uniformly dispersed with water to obtain a slurry with a solid content of 1.9%. The slurry is poured into a sheet maker, and after the slurry is uniformly dispersed, it is vacuum dehydrated to a solid content of 10-25% under a vacuum degree of 0.01-0.06MPa, and then further dehydrated with a press to obtain a wet paper web with a moisture content of 43%, which is placed in a 105°C drying cylinder for drying to obtain base paper. Aluminum hydroxide is ground in a ball mill for 30 minutes, the diameter of the grinding beads is 1-2mm, and the ball-to-material ratio is 25:1 to obtain aluminum hydroxide particles with an average particle size of 90nm. The aluminum hydroxide particles are added to a phenolic resin ethanol solution with a solid content of 34%, first ultrasonically treated for 15 minutes, and then mechanically stirred for 30 minutes to obtain a phenolic resin impregnation solution. The base paper was immersed in the above phenolic resin dipping solution at room temperature for 10 minutes, taken out, and dried at 80°C for 40 minutes to obtain the dipped paper with a glue content of 33.1%. The dipped paper was placed on a vulcanizer and hot-pressed and vulcanized at 200°C and 4MPa for 3 minutes to obtain a high-porosity wet paper-based friction material. The quantitative value of the high-porosity wet paper-based friction material is 345g / m 2 , with a thickness of 416 μm. The mass of aluminum hydroxide particles accounts for 3% of the dry weight of the phenolic resin.
[0113] The porosity of the high-porosity wet paper-based friction material was measured by a fully automatic true density analyzer to be 46.8%, and the average pore size of the material was measured by a Capillary Flow Porometer to be 2.3325 μm. The pore size distribution is as follows: Figure 6 shown.
[0114] The friction and wear performance of the high-porosity wet paper-based friction material was tested using an MM2000 friction performance tester. Under the conditions of a rotation speed of 2000r / min and a pressure of 0.4MPa, the dynamic friction coefficient of the high-porosity wet paper-based friction material was 0.121, which was 27.4% higher than that of comparative example 2; the static friction coefficient was 0.134, which was 26.4% higher than that of comparative example 2. It meets the requirements of Class 2 and Class 3 products in the national standard GB / T37208-2018 non-metallic paper-based wet friction materials.
[0115] Comparative Example 3
[0116] By weight, 20 parts of cotton fiber, 10 parts of aramid fiber, 10 parts of carbon fiber, 30 parts of diatomaceous earth, 5 parts of feldspar, 5 parts of barium sulfate, 10 parts of graphite, and 10 parts of rubber powder are uniformly dispersed with water to obtain a slurry with a solid content of 2%. The slurry is poured into a sheet maker, and after the slurry is uniformly dispersed, it is vacuum dehydrated to a solid content of 10-25% under a vacuum degree of 0.01-0.06MPa, and then further dehydrated with a press to obtain a wet paper web with a moisture content of 43%, which is placed in a 105°C drying cylinder for drying to obtain base paper. The base paper is placed in a phenolic resin ethanol solution with a solid content of 27%, dipped in glue at room temperature for 10 minutes, taken out, and dried at 85°C for 30 minutes to obtain dipped paper with a glue content of 28.9%. The dipped paper is placed on a vulcanizer and hot-pressed and vulcanized for 5 minutes at 210°C and 3MPa to obtain a high-porosity wet paper-based friction material. The basis weight of the high porosity wet paper-based friction material is 345g / m 2 , thickness is 380μm.
[0117] The porosity of the high-porosity wet paper-based friction material was measured by a fully automatic true density analyzer to be 41.7%, and the average pore size of the material was measured by a Capillary Flow Porometer to be 1.8635 μm. The pore size distribution is as follows: Figure 7 shown.
[0118] The friction and wear properties of the high-porosity wet paper-based friction material were tested using an MM2000 friction performance tester. Under the conditions of a rotation speed of 2000 r / min and a pressure of 0.4 MPa, the dynamic friction coefficient of the wet paper-based friction material was 0.106 and the static friction coefficient was 0.112. After 2000 tests, the wear rate was 3×10 -7 cm 2 / J. It meets the requirements of Class 2 and Class 3 products in the national standard GB / T37208-2018 non-metallic paper-based wet friction materials.
[0119] Example 5
[0120] In terms of mass, 8 parts of cotton fiber, 8 parts of aramid fiber, 8 parts of carbon fiber, 15 parts of diatomaceous earth, 5 parts of feldspar, 6 parts of graphite, 30 parts of rubber, and 20 parts of friction powder are uniformly dispersed with water to obtain a slurry with a solid content of 1.7%. A 3wt% aluminum sulfate aqueous solution is added to the slurry until the pH value of the system reaches 3.0, and stirred for 10 minutes; a 5wt% sodium hydroxide aqueous solution is added to adjust the pH value of the system to 7.0, and stirred for 10 minutes. The prepared slurry is poured into a sheet making machine, and after the slurry is uniformly dispersed, vacuum dehydration is performed under a vacuum degree of 0.01-0.06MPa to a solid content of 10-25%, and then a press is used to further remove water to obtain a wet paper web with a moisture content of 42%, which is placed in a 95°C vacuum dryer and dried for 5 minutes to obtain base paper. The base paper was immersed in a phenolic resin ethanol solution with a solid content of 30% for 10 minutes, taken out, and dried at 105°C for 10 minutes to obtain a dipped paper with a glue content of 29.2%. The dipped paper was placed on a vulcanizer for hot pressing, and vulcanized and hot pressed at 200°C and 2MPa for 5 minutes to obtain a high-porosity wet paper-based friction material. The quantitative value of the high-porosity wet paper-based friction material is 410g / m 2 , thickness is 386μm.
[0121] The porosity of the high-porosity wet paper-based friction material was measured by a fully automatic true density analyzer to be 25.1%, and the average pore size of the material was measured by a Capillary Flow Porometer to be 3.1700 μm. The pore size distribution is as follows: Figure 8 shown.
[0122] The friction and wear properties of the high-porosity wet paper-based friction material were tested using an MM2000 friction performance tester. Under the conditions of a rotation speed of 2000 r / min and a pressure of 0.4 MPa, the dynamic friction coefficient of the material was 0.094, which was 11.9% higher than that of comparative example 1; the static friction coefficient was 0.113, which was 18.9% higher than that of comparative example 1; the wear rate was 4×10 -7 cm2 / J, which is 20% lower than that of comparative example 1; it meets the requirements of Class 2 and Class 3 products in the national standard GB / T37208-2018 non-metallic paper-based wet friction materials.
[0123] Example 6
[0124] In terms of mass, 8 parts of cotton fiber, 8 parts of aramid fiber, 8 parts of carbon fiber, 15 parts of diatomaceous earth, 5 parts of feldspar, 6 parts of graphite, 30 parts of rubber, and 20 parts of friction powder are uniformly dispersed with water to obtain a slurry with a solid content of 1.7%. A 15wt% aluminum sulfate aqueous solution is added to the slurry until the pH value of the system reaches 1.0, and stirred for 5 minutes; a 20wt% sodium hydroxide aqueous solution is added to adjust the pH value of the system to 7.3, and stirred for 15 minutes. The prepared slurry is poured into a sheet making machine, and after the slurry is uniformly dispersed, vacuum dehydration is performed under a vacuum degree of 0.01-0.06MPa to a solid content of 10-25%, and then a press is used to further remove water to obtain a wet paper web with a moisture content of 42%, which is placed in a 105°C oven for drying for 5 minutes to obtain base paper. The base paper was immersed in a phenolic resin ethanol solution with a solid content of 33% for 15 minutes, then taken out and dried at 105°C for 10 minutes to obtain a dipped paper with a glue content of 32.4%. The dipped paper was placed on a vulcanizer and vulcanized and hot-pressed at 210°C and 2.2MPa for 10 minutes to obtain a high-porosity wet paper-based friction material. The quantitative value of the high-porosity wet paper-based friction material is 400g / m 2 , thickness is 398μm.
[0125] The porosity of the high-porosity wet paper-based friction material was measured by a fully automatic true density analyzer to be 26.9%, and the average pore size of the material was measured by a Capillary Flow Porometer to be 3.4131 μm. The pore size distribution is as follows: Fig. 9 shown.
[0126] The friction and wear properties of the high-porosity wet paper-based friction material were tested using an MM2000 friction performance tester. Under the conditions of a rotation speed of 2000 r / min and a pressure of 0.4 MPa, the dynamic friction coefficient of the material was 0.108, which was 28.6% higher than that of comparative example 1; the static friction coefficient was 0.109, which was 14.7% higher than that of comparative example 1; the wear rate was 3×10 -7 cm 2 / J, which is reduced by 40% compared with Comparative Example 1.
[0127] Example 7
[0128] In terms of mass, 8 parts of cotton fiber, 8 parts of aramid fiber, 8 parts of carbon fiber, 15 parts of diatomaceous earth, 5 parts of feldspar, 6 parts of graphite, 30 parts of rubber, and 20 parts of friction powder are uniformly dispersed with water to obtain a slurry with a solid content of 1.8%. 2 parts of 800 mesh aluminum hydroxide are added to the slurry and stirred for 20 minutes. The prepared slurry is poured into a sheet maker. After the slurry is uniformly dispersed, it is vacuum dehydrated to a solid content of 10-25% under a vacuum degree of 0.01-0.06MPa, and then further dehydrated with a press to obtain a wet paper web with a moisture content of 42%, which is placed in a 105°C drying cylinder and dried for 5 minutes to obtain base paper. The base paper is placed in a phenolic resin ethanol solution with a solid content of 34% and immersed for 15 minutes, then taken out, and dried at 90°C for 30 minutes to obtain a dipped paper with a glue content of 31.7%. The impregnated paper was placed on a vulcanizer and vulcanized and hot-pressed for 3 minutes at 210°C and 3MPa to obtain a high-porosity wet paper-based friction material. The quantitative value of the high-porosity wet paper-based friction material is 409g / m 2 , thickness is 412μm.
[0129] The porosity of the high-porosity wet paper-based friction material measured by a full-automatic true density analyzer is 24.5%, which is 6.5% higher than that of comparative example 1; the average pore diameter is 3.1879 μm, which is 6% higher than that of comparative example 1.
[0130] The friction and wear properties of the high-porosity wet paper-based friction material were tested using an MM2000 friction performance tester. Under the conditions of a rotation speed of 2000 r / min and a pressure of 0.4 MPa, the dynamic friction coefficient of the material was 0.096, which was 14.3% higher than that of comparative example 1; the static friction coefficient was 0.108, which was 13.7% higher than that of comparative example 1; and the wear rate was 4.5×10 -7 cm2 / J, which is reduced by 10% compared with Comparative Example 1.
[0131] Example 8
[0132] In terms of mass, 20 parts of cotton fiber, 10 parts of aramid fiber, 10 parts of carbon fiber, 30 parts of diatomaceous earth, 5 parts of feldspar, 5 parts of barium sulfate, 10 parts of graphite, and 10 parts of rubber are uniformly dispersed with water to obtain a slurry with a solid content of 1.8%. A 25wt% aluminum sulfate aqueous solution is added to the slurry until the pH value of the system is 0.7, and stirred for 15 minutes; a 30wt% sodium hydroxide aqueous solution is added to adjust the pH value of the system to 7.2, and stirred for 15 minutes. The prepared slurry is poured into a sheet making machine, and after the slurry is uniformly dispersed, vacuum dehydration is performed under a vacuum degree of 0.01-0.06MPa to a solid content of 10-25%, and then a press is used to further remove water to obtain a wet paper web with a moisture content of 43%, which is placed in a 105°C drying cylinder for 6 minutes to obtain base paper. The base paper was immersed in a phenolic resin ethanol solution with a solid content of 27% for 10 minutes, then taken out and dried at 85°C for 30 minutes to obtain a dipped paper with a glue content of 28.6%. The dipped paper was placed on a vulcanizer and vulcanized and hot-pressed at 210°C and 3MPa for 5 minutes to obtain a high-porosity wet paper-based friction material. The quantitative weight of the high-porosity wet paper-based friction material is 341g / m 2 , thickness is 379μm.
[0133] The porosity of the high-porosity wet paper-based friction material measured by a full-automatic true density analyzer is 44.3%, which is 6.2% higher than that of comparative example 3; the average pore diameter is 2.3524 μm, which is 26.2% higher than that of comparative example 3.
[0134] The friction and wear properties of the high-porosity wet paper-based friction material were tested using an MM2000 friction performance tester. Under the conditions of a rotation speed of 2000 r / min and a pressure of 0.4 MPa, the dynamic friction coefficient of the material was 0.108, which was 1.9% higher than that of comparative example 3; the static friction coefficient was 0.130, which was 16.1% higher than that of comparative example 3; the wear rate was 2×10 -7 cm2 / J, which is reduced by 50% compared with Comparative Example 3.
[0135] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a high-porosity wet paper-based friction material, comprising the following steps: mixing natural fibers, synthetic fibers, friction modifier fillers and water to obtain a slurry; Dehydrating the slurry, forming it, and then drying it to obtain base paper; The base paper is impregnated in a phenolic resin impregnation solution and then dried to obtain impregnated paper; The impregnated paper is subjected to hot pressing and vulcanization to obtain a high-porosity wet-type paper-based friction material; The slurry or the phenolic resin dipping solution also includes a pore-forming agent; The pore-forming agent in the slurry includes a water-soluble pore-forming agent and an inorganic strong base, or an insoluble pore-forming agent; the water-soluble pore-forming agent includes aluminum sulfate, or alum and sulfuric acid; the insoluble pore-forming agent includes aluminum hydroxide particles and / or calcium oxalate powder, and the pH value of the slurry containing the inorganic strong base is 6 to 8; The pore-forming agent in the phenolic resin dipping solution includes one or more of aluminum hydroxide particles, alum and calcium oxalate powder.
2. The high porosity wet paper-based friction material according to claim 1, characterized in that: When the slurry further includes aluminum sulfate and an inorganic strong base, the preparation method of the slurry containing a pore-forming agent comprises the following steps: adding aluminum sulfate to the slurry until the pH value is 0.1 to 5, and then adding an inorganic strong base to adjust the pH value to 6 to 8; When the slurry further includes alum, sulfuric acid and an inorganic strong base, the preparation method of the slurry containing a pore-forming agent comprises the following steps: adding alum to the slurry, adding sulfuric acid to adjust the pH value to 0.1-5, and then adding an inorganic strong base to adjust the pH value to 6-8; the mass of alum in the slurry accounts for 0.1-5% of the dry weight of the slurry without adding the insoluble pore-forming agent; When the slurry further includes an insoluble pore former, the preparation method of the slurry containing the pore former includes the following steps: adding the insoluble pore former to the slurry; the mass of the insoluble pore former accounts for 0.001-10% of the mass of the slurry without the insoluble pore former.
3. The high porosity wet paper-based friction material according to claim 1, characterized in that: When the phenolic resin dipping solution further includes a pore-forming agent, the mass of the pore-forming agent accounts for 0.1-5% of the dry weight of the phenolic resin, and the particle size of the pore-forming agent is 1-1000 nm.
4. The preparation method according to claim 1 or 3, characterized in that: The phenolic resin in the phenolic resin dipping solution includes one or more of unmodified phenolic resin, cashew nut shell oil modified phenolic resin, melamine modified phenolic resin, latex modified phenolic resin and boron modified phenolic resin; The solid content of the phenolic resin dipping solution is 20-50%.
5. The high-porosity wet paper-based friction material according to claim 1 or 2, characterized in that: The natural fibers include one or more of hemp fibers, cotton fibers, bamboo fibers and wood pulp fibers; The synthetic fiber includes one or more of aramid fiber, carbon fiber, glass fiber, ceramic fiber and polyimide fiber; The friction performance modifier filler includes one or more of diatomaceous earth, silicon dioxide, feldspar, barium sulfate, graphite, aluminum oxide and organic friction powder; The mass ratio of the natural fiber to the synthetic fiber is 1:0.1-8; The mass ratio of the natural fiber to the friction performance modifier filler is 1:0.1-12; The solid content of the slurry is 0.5-3%.
6. The preparation method according to claim 1, characterized in that: The dipping time is 3 to 20 minutes.
7. The preparation method according to claim 1, characterized in that: The temperature of the hot pressing vulcanization is 180-230° C., the pressure is 1-30 MPa, and the time is 1-30 min.
8. A high-porosity wet paper-based friction material prepared by the preparation method according to any one of claims 1 to 7.
9. The preparation method according to claim 8, characterized in that: The quantitative weight of the high-porosity wet paper-based friction material is 100-2000 g / m 2 , thickness is 0.2~5mm.
10. Use of the high-porosity wet paper-based friction material according to claim 8 or 9 in a wet clutch or wet brake device.
Citation Information
Patent Citations
Thermal-decomposing pore-forming self-heat-insulating bearing sintered product and preparation method thereof
CN101644088A
Wet type paper-based friction material as well as preparation method and application thereof
CN102002883A
Preparation method for ceramic film with hierarchical pore structure
CN102701778A
Carbon fiber brake pad material with porous structure and preparation method of carbon fiber brake pad material
CN108662050A
Preparation method of cross-linked hydrotalcite, water-based coating and preparation method of water-based coating
CN110182833A