Maintenance construction method for small box girder wet joint cracking white precipitation disease

By applying a multi-layered coating of cement-based penetrating crystallizing material, interface agent, and polymer repair mortar, the problem of poor repair effect of cracking and whitening defects in wet joints of small box girders was solved, and the mechanical properties and durability were improved, preventing secondary cracking.

CN118911044APending Publication Date: 2024-11-08LUPU BRIDGE MAINTENANCE & MANAGEMENT BRANCH SHANGHAI MUNICIPAL CONSERVATION MANAGEMENT +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410578114.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-10
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing technology lacks standardized materials and construction methods for repairing cracks and whitening defects in wet joints of small box girders, resulting in poor repair results and a high risk of secondary cracking.

Method used

A specific application sequence of cement-based penetrating crystallizing material, interface agent, and polymer repair mortar is used, including the steps of roughening, applying cement-based penetrating crystallizing material, water curing, applying interface agent, and applying polymer repair mortar to form a multi-layer repair structure.

Benefits of technology

It significantly improves the flexural strength, compressive strength, impact toughness, bonding performance, and frost resistance of the repair area, prevents secondary cracking, and enhances the mechanical properties and durability of the wet joints of the small box girder.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118911044A_ABST
    Figure CN118911044A_ABST
Patent Text Reader

Abstract

The invention provides a small box girder wet joint cracking white precipitation disease maintenance construction method. According to the invention, three materials, namely the cement-based capillary crystalline material, the interface agent and the polymer repairing mortar, are used for repairing the cracking white-out damage of the small box girder, and the brushing sequence of the three materials is determined; the breaking strength, the compressive strength, the impact toughness, the bonding performance, the freezing resistance and the anti-permeability of a maintenance area are improved compared with those of a maintenance area using a mud-based capillary crystalline material or a polymer repair mortar single-layer material, and the mechanical property and the durability of an original crack area are greatly improved. According to the method, the secondary cracking phenomenon of a maintenance area under the action of rain wash, variable loads and repeated moving loads in the flood season can be effectively prevented, a complete construction method is provided for small box girder wet joint cracking white precipitation maintenance, design is scientific, operation is easy, and the method has extremely high popularization value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of bridge maintenance, and in particular relates to a repair construction method for cracking and whitening defects of wet joints of small box girders. Background Art

[0002] The main line elevated superstructure under the jurisdiction of S7 Shanghai-Chongqing Expressway (Phase I) mainly adopts prefabricated small box girders (C50) with a span of about 30m made of simply supported prestressed concrete. The wet joints are cast-in-place with high-performance concrete (C80) with a width of 30cm and staggered steel bars without welding. According to the inspection results of regular inspection reports, daily inspections and regular inspections from 2021 to 2022, transverse cracking and whitening are common in the wet joints of prefabricated beams. The development speed is relatively fast, from 79 in 2021 to 135 in 2022. This problem is largely caused by the construction process of prefabrication and assembly first and then pouring wet joints. Due to the different concrete construction times of the prefabricated box girder part and the cast-in-place wet joint part, when the cast-in-place concrete of the wet joint shrinks, it is easy to cause transverse cracking in the wet joint due to the constraints of the prefabricated beams on both sides.

[0003] At present, there is no standard for the repair materials and methods of prefabricated small box beam wet joint cracking in China, and the actual repair results are uneven. Construction units often use cement-based penetrating crystallization materials or polymer repair mortar materials for repair. After the repair, secondary cracks will still occur in the original area within a short period of time, resulting in whitening phenomenon, which makes secondary repair more difficult.

[0004] In order to ensure that the bridge structure is always in a stable and good technical state and maintain its safety and durability, a centralized maintenance project is planned for the wet joint crack disease of small box girders. Therefore, a repair construction method for the wet joint cracking and whitening disease of small box girders is urgently needed. Summary of the invention

[0005] The present invention is made to solve the above-mentioned problem and aims to provide a repair construction method for cracking and whitening defects of wet joints of small box beams.

[0006] The invention provides a repair construction method for cracking and whitening defects of wet joints of small box girders, which is used for repairing cracks at cracks of wet joints of small box girders and has the following characteristics, comprising the following steps: S10, roughening concrete in a certain area where the cracks are located to form a roughened area, and then cleaning the roughened area; S20, brushing a cement-based penetrating crystallization material on the roughened area and completely covering it to form a cement-based penetrating crystallization material coating; S30, spraying water on the cement-based penetrating crystallization material coating for curing; S40, when the cement-based penetrating crystallization material coating is condensed but still sticky, brushing an interface agent on it and completely covering it to form an interface agent coating; S50, after the interface agent coating is initially solidified and the surface becomes sticky, applying a polymer repair mortar on the interface agent coating and completely covering it to form a polymer repair mortar coating; S60, completing the construction after curing the polymer repair mortar coating.

[0007] In the small box girder wet joint cracking and whitening disease repair construction method provided by the present invention, it can also have the following characteristics: wherein, in step S10, the roughening method is: use a chisel or a small electric hammer to chisel off the hardened latex on the concrete surface in a certain area above and around the crack to form a rough surface, and the cleaning method is: use a high-pressure water gun to spray the roughened area to ensure that the alkali, dust, paint and film in the roughened area are removed, so that the base surface is fully moistened, and then wipe off the clear water on the surface of the roughened area.

[0008] The small box girder wet joint cracking and whitening defect repair construction method provided by the present invention may also have the following characteristics: wherein, in step S10, the depth of roughening is such that 1 / 3 to 1 / 2 of the gravel in the concrete in the roughening area is exposed, and the shortest distance from any position on the edge of the roughening area to any position on the crack is 5 to 8 cm.

[0009] The small box girder wet joint cracking and whitening defect repair construction method provided by the present invention may also have the following characteristics: wherein, in step S20, a semi-hard nylon brush is used to apply cement-based penetrating crystallization material, the cement-based penetrating crystallization material coating covers the roughened area and the edge of the cement-based penetrating crystallization material coating exceeds the edge of the roughened area by 2 to 3 cm.

[0010] The small box girder wet joint cracking and whitening disease repair construction method provided by the present invention may also have the following characteristics: wherein, in step S20, the cement-based infiltration crystallization material is a gray powdery inorganic material composed of cement, silica sand and a variety of active chemical substances, the active chemical substance is a calcium complex, and the amount of the cement-based infiltration crystallization material is 1 to 1.5 kg / m 2 .

[0011] The small box girder wet joint cracking and whitening defect repair construction method provided by the present invention may also have the following characteristics: wherein, in steps S30 to S40, after curing the cement-based penetrable crystalline material coating, wait for at least 6 hours before applying the interface agent, and the method of applying the interface agent is: use a roller to apply 2 to 3 times, the interface agent coating covers the cement-based penetrable crystalline material coating and the edge of the interface agent coating exceeds the edge of the cement-based penetrable crystalline material coating by 2 to 3 cm.

[0012] The small box girder wet joint cracking and whitening defect repair construction method provided by the present invention may also have the following characteristics: wherein, in step S40, the interface agent is a modified acrylic acid solution, and the modified acrylic acid solution is an emulsion-like substance prepared by emulsification reaction of acrylic acid and a modifier by an emulsion polymerization method.

[0013] The small box girder wet joint cracking and whitening defect repair construction method provided by the present invention may also have the following characteristics: wherein, in step S50, the method of applying the polymer repair mortar is: using a spatula, a trowel or a gloved hand to carry out the coating construction, the polymer repair mortar coating covers the interface agent coating and the edge of the polymer repair mortar coating exceeds the interface agent coating by 2 to 3 cm.

[0014] The small box girder wet joint cracking and whitening disease repair construction method provided by the present invention may also have the following characteristics: wherein, in step S50, the polymer repair mortar is a new type of concrete repair mortar, the new type of concrete repair mortar has both the adhesion of polymer materials and the durability of inorganic materials, and the thickness of the polymer repair mortar coating is 4 to 6 mm.

[0015] The small box girder wet joint cracking and whitening defect repair construction method provided by the present invention may also have the following characteristics: wherein, in step S60, the curing method is: 24 hours after construction, covering the polymer repair mortar coating with plastic sheet for wet curing for at least 7 days, and regularly sprinkling water for curing.

[0016] Functions and Effects of the Invention

[0017] The repair construction method for wet joint cracking and whitening defects of small box girders according to the present invention is used to repair cracks at wet joint cracking of small box girders. Since three materials, cement-based penetrating crystallization material, interface agent and polymer repair mortar, are used to repair the cracking and whitening defects of small box girders, the painting order of the three materials is determined, so that the flexural strength, compressive strength, impact toughness, bonding performance, frost resistance and impermeability of the repair area are improved compared with the repair using mud-based penetrating crystallization material or polymer repair mortar single-layer material, and the mechanical properties and durability of the original crack area are greatly improved.

[0018] The present invention can effectively prevent secondary cracking in the maintenance area under the effects of rain scouring during the flood season, variable loads and repeated moving loads, and proposes a complete construction method for the crack analysis and repair of wet joints of small box girders. The design is scientific and the operation is simple, and the promotion value is extremely high. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 It is a flowchart of a repair construction method for a small box girder wet joint cracking and whitening disease according to an embodiment of the present invention;

[0020] Figure 2 It is a top view schematic diagram of the construction process of the small box girder wet joint cracking and whitening disease repair construction method according to an embodiment of the present invention;

[0021] Figure 3 yes Figure 2 The main view section corresponding to part (e) in FIG. DETAILED DESCRIPTION

[0022] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the following embodiments and the accompanying drawings specifically illustrate a small box girder wet joint cracking and whitening disease repair construction method of the present invention.

[0023] <Example>

[0024] Figure 1 It is a flowchart of a repair construction method for a small box girder wet joint cracking and whitening disease according to an embodiment of the present invention; Figure 2 It is a top view schematic diagram of the construction process of the small box girder wet joint cracking and whitening disease repair construction method according to an embodiment of the present invention; Figure 3 yes Figure 2 The main view section corresponding to part (e) in FIG.

[0025] like Figures 1 to 3 As shown, this embodiment provides a small box girder wet joint cracking and whitening disease repair construction method, which is used to repair the crack 1 at the small box girder wet joint cracking, including the following steps:

[0026] S10, such as Figure 2 As shown in part (a) of the diagram, there is a 0.4 mm wide crack 1 at the crack of the small box beam wet joint. Use a chisel or a small electric hammer to chisel away the hardened latex on the surface of the concrete 2 above and around the crack 1 to form a rough surface, as shown in the figure. Figure 2 The roughened area 10 is shown in part (b) of FIG.

[0027] The roughened area 10 is a rectangle, and the shortest distance between any position on the rectangle and any position on the crack 1 is 5 cm. The depth of the roughened area 10 is chiseled so that 1 / 3 to 1 / 2 of the gravel in the concrete of the roughened area 10 is exposed.

[0028] Subsequently, the roughened area 10 is sprayed with a high-pressure water gun to remove efflorescence, dust, paint and film in the roughened area 10 , and after the base surface is fully moistened, a towel is used to wipe off the clear water on the surface of the roughened area 10 .

[0029] S20, use a semi-hard nylon brush to vigorously brush vertically and horizontally to completely cover the chiseled area 10 with the cement-based infiltration crystallization material and the coverage exceeds 2 cm, forming a Figure 2 Part (c) of Figure 3 A cementitious permeable crystalline material coating 20 is shown.

[0030] Among them, cement-based permeable crystallization material is a gray powdery inorganic material composed of cement, silica sand and a variety of active chemical substances (calcium complexes). The amount of brushing should be strictly used according to the instructions of the material, which is 1-1.5 kg / m 2 .

[0031] S30, spraying and curing the cement-based penetrating crystalline material coating 20 with mist water.

[0032] S40, wait for 6 hours until the cement-based penetrating crystallization material coating 20 solidifies, touch it with your hand to confirm that it still has a certain viscosity, record the time, and then use a roller to brush the interface agent twice to completely cover the cement-based penetrating crystallization material coating 20 and the coverage range exceeds it by 2 cm, forming a Figure 2 Part (d) of Figure 3 An interface agent coating 30 is shown.

[0033] The interfacial agent is a modified acrylic acid solution, which is an emulsion-like substance prepared by an emulsion polymerization method through an emulsification reaction of acrylic acid and a modifier.

[0034] In this step, the time is recorded to facilitate quantification of the specific construction time in the area and climate conditions to facilitate the next construction.

[0035] S50, after the moisture of the interface agent coating 30 evaporates, the slurry is initially set, and the surface is confirmed to be sticky by touching it with hands, the polymer repair mortar is spread by a spatula, a trowel or a hand with gloves to completely cover the interface agent coating 30 and the coverage range exceeds 2 cm, forming a Figure 2 Part (e) of Figure 3 The polymer repair mortar coating 40 is shown to have a thickness of 6 mm.

[0036] In this step, the time for waiting for the moisture in the interface agent coating 30 to evaporate and the slurry to initially set is at least 30 minutes, and specific adjustments are made according to the weather temperature during construction.

[0037] Among them, polymer repair mortar is a new type of concrete repair mortar that combines the adhesion of polymer materials and the durability of inorganic materials.

[0038] S60, 24 hours after construction, cover the polymer repair mortar coating 40 with plastic sheeting and maintain in a wet state for 7 days, and regularly sprinkle water for maintenance, and finally complete the construction.

[0039] In this embodiment, the cement-based penetrating crystallization material, the interface agent and the polymer repair mortar are all directly purchased finished products under the existing technology.

[0040] Functions and Effects of the Embodiments

[0041] According to a repair construction method for cracking and whitening defects of wet joints of small box girders provided in this embodiment, the method is used to repair cracks at cracks in wet joints of small box girders, and comprises the following steps: S10, roughening the concrete in a certain area where the cracks are located to form a roughened area, and then cleaning the roughened area; S20, applying a cement-based penetrating crystalline material on the roughened area and completely covering it to form a cement-based penetrating crystalline material coating; S30, spraying water on the cement-based penetrating crystalline material coating for curing; S40, when the cement-based penetrating crystalline material coating is solidified but still sticky, applying an interface agent on it and completely covering it to form an interface agent coating; S50, after the interface agent coating is initially solidified and the surface becomes sticky, applying a polymer repair mortar on the interface agent coating and completely covering it to form a polymer repair mortar coating; S60, completing the construction after curing the polymer repair mortar coating. Therefore, this embodiment determines the brushing order of the three materials of cement-based penetrating crystallization material, interface agent and polymer repair mortar, so that the flexural strength, compressive strength, impact toughness, bonding performance, frost resistance and impermeability of the repair area are improved compared with the repair using mud-based penetrating crystallization material or polymer repair mortar single-layer material, and greatly improves the mechanical properties and durability of the original crack area. In addition, this embodiment can effectively prevent the repair area from secondary cracking under the action of rainwater scouring, variable load and repeated moving load during the flood season, and proposes a complete set of construction methods for crack analysis and repair of small box beam wet joints. The design is scientific and the operation is simple, which has a very high promotion value.

[0042] Furthermore, in step S10, the roughening method is: use a chisel or a small electric hammer to chisel off the hardened latex on the concrete surface above the crack and a certain area around it to form a rough surface, and the cleaning method is: use a high-pressure water gun to spray the roughened area to ensure that the alkali, dust, paint and film in the roughened area are removed, so that the base surface is fully moistened, and then wipe off the clear water on the surface of the roughened area. The advantages of such operation are: 1. Increase the contact surface and provide sufficient penetration capillary channels, which is more conducive to the penetration and crystallization of the cement-based penetrating crystallization material in step S20, and give full play to the material function; 2. Provide a solid bonding foundation for the cement-based penetrating crystallization material coating in step S20, and increase the inward integrity of the repair structure in the case of top surface construction.

[0043] Furthermore, in step S10, if the roughening is too deep, the original concrete structure will be damaged and materials will be wasted, which is not worth the loss; if it is too shallow, the roughening effect cannot be achieved and the expected repair effect cannot be achieved. Therefore, the roughening depth is such that 1 / 3 to 1 / 2 of the stones in the concrete in the roughening area are exposed, and the shortest distance from any position on the edge of the roughening area to any position on the crack is 5 cm. Such operation makes the subsequent construction more orderly and efficient, improves the construction accuracy, rationally uses materials and saves construction costs.

[0044] Furthermore, in step S20, a semi-hard nylon brush is used to brush the cement-based penetrating crystallization material vertically and horizontally, and the cement-based penetrating crystallization material coating covers the roughened area and the edge of the cement-based penetrating crystallization material coating exceeds the edge of the roughened area by 2 cm. The advantages of this operation are: 1. Vertical and horizontal brushing allows as much cement-based penetrating crystallization material as possible to be brushed into the cracks, better exerting the plugging effect of penetrating crystallization to repair the cracks, which is crucial in the subsequent self-healing of the cracks (exerting the self-healing properties of subsequent cracks); 2. Vertical and horizontal brushing ensures that the penetrating crystallization material is fully in contact with the roughened area and is evenly applied; 3. Exceeding the edge by a certain range can ensure that the original performance of the roughened area is not damaged, while better realizing the integrity of the cement-based penetrating crystallization material coating and the roughened area.

[0045] Furthermore, in step S20, the cement-based infiltration crystallization material is a gray powder inorganic material composed of cement, silica sand and a variety of special active chemical substances (calcium complexes), and the amount of the cement-based infiltration crystallization material is 1-1.5 kg / m 2. In this embodiment, the amount of cement-based permeable crystallization material determines the thickness of the cement-based permeable crystallization material coating. And the unique active chemical substances in the cement-based permeable crystallization material utilize the inherent chemical properties and porosity of cement concrete itself, use water as a carrier, and rely on osmosis to transmit and fill in the concrete micropores and capillaries, catalyzing the particles and incompletely hydrated components in the concrete to undergo hydration again to form insoluble dendrite-like crystals and combine with the concrete to form a whole, so that water and other liquids coming from any direction are blocked to achieve permanent waterproofing, moisture-proofing, protection of steel bars and enhancement of concrete structure strength. It has the characteristics and performance of multiple anti-seepage and self-repair, and has extremely strong compressive resistance.

[0046] Furthermore, in steps S30 to S40, after curing the cement-based infiltrative crystallization material coating, wait for at least 6 hours before applying the interface agent. The method of applying the interface agent is: use a roller to apply twice, the interface agent coating covers the cement-based infiltrative crystallization material coating and the edge of the interface agent coating exceeds the edge of the cement-based infiltrative crystallization material coating by 2 cm. The advantages of this operation are: 1. Applying twice ensures that the interface agent plays a corresponding role without waste; 2. Ensures the firm bonding of the cement-based infiltrative crystallization material coating and the polymer repair mortar in step S50, and improves the internal integrity of the repair structure.

[0047] Furthermore, in step S40, the interface agent is a modified acrylic acid solution, which is an emulsion-like substance prepared by an emulsion polymerization method through an emulsion reaction of acrylic acid and a modifier. In this embodiment, the interface agent has good stability, is not easy to gel or precipitate, has good weather resistance, is not easily affected by external environments such as oxidation, hydrolysis and light, has good adhesion to a variety of surface materials, can form a uniform and firm film on different surfaces, has good water resistance, is not easily eroded and damaged by water, and has two-way permeability and adhesion.

[0048] Furthermore, in step S50, the method of applying the polymer repair mortar is: using a spatula, a trowel or a gloved hand to apply the polymer repair mortar coating, the polymer repair mortar coating covers the interface agent coating and the edge of the polymer repair mortar coating exceeds the interface agent coating by 2 cm. The advantage of this operation is that the polymer repair mortar is evenly applied and the cement penetration crystallization material coating is protected.

[0049] Furthermore, in step S50, the polymer repair mortar is a new type of concrete repair mortar, which has both the adhesion of polymer materials and the durability of inorganic materials, and the thickness of the polymer repair mortar coating is 6 mm. In this way, the optimal thickness of the polymer repair mortar coating is determined.

[0050] Furthermore, in step S60, the curing method is: 24 hours after construction, cover the polymer repair mortar coating with plastic sheeting for 7 days of wet curing, and regularly sprinkle water for curing. The advantages of this operation are: the polymer repair mortar coating does not crack, achieves the expected strength, better protects its internal coating, prevents secondary cracking, and improves the internal integrity of the repair structure.

[0051] Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A small box girder wet joint cracking and whitening disease repair construction method, used to repair the cracks at the small box girder wet joint cracking, It is characterized in that The following steps are involved: S10, roughening the concrete in a certain area where the crack is located to form a roughened area, and then cleaning the roughened area; S20, applying a cement-based infiltrative crystallization material on the roughened area and completely covering it to form a cement-based infiltrative crystallization material coating; S30, spraying water to cure the cement-based permeable crystalline material coating; S40, when the cement-based permeable crystalline material coating is solidified but still sticky, applying an interface agent thereon and completely covering it to form an interface agent coating; S50, after the interface agent coating is initially solidified and the surface becomes sticky, a polymer repair mortar is applied on the interface agent coating and completely covers it to form a polymer repair mortar coating; S60, completing the construction after curing the polymer repair mortar coating.

2. The repair construction method for cracking and whitening defects of small box beam wet joints according to claim 1 is characterized by: in, In step S10, the roughening method is: using a chisel or a small electric hammer to chisel away the hardened latex on the concrete surface in a certain area above and around the crack to form a rough surface. The cleaning method is: use a high-pressure water gun to spray the roughened area to ensure that the alkali, dust, paint and film in the roughened area are removed, so that the base surface is fully wetted, and then wipe off the clear water on the surface of the roughened area.

3. The repair construction method for small box beam wet joint cracking and whitening disease according to claim 1 or 2, characterized in that: in, In step S10, the depth of roughening is such that 1 / 3 to 1 / 2 of the gravel in the concrete in the roughening area is exposed. The shortest distance between any position on the edge of the roughened area and any position on the crack is 5 to 8 cm.

4. The repair construction method for cracking and whitening defects of wet joints of small box beams according to claim 1 is characterized in that: in, In step S20, a semi-hard nylon brush is used to apply the cement-based infiltration crystallization material. The cement-based infiltrative crystalline material coating covers the roughened area, and the edge of the cement-based infiltrative crystalline material coating exceeds the edge of the roughened area by 2 to 3 cm.

5. The repair construction method for small box beam wet joint cracking and whitening disease according to claim 1 or 4, characterized in that: in, In step S20, the cement-based infiltration crystallization material is a gray powdery inorganic material composed of cement, silica sand and a variety of active chemical substances. The active chemical substance is a calcium complex, The amount of cement-based infiltration crystallization material is 1-1.5 kg / m 2 .

6. The repair construction method for cracking and whitening defects of wet joints of small box beams according to claim 1 is characterized by: in, In steps S30 to S40, the interface agent is applied after curing the cement-based permeable crystallization material coating for at least 6 hours. The method of applying the interface agent is: use a roller to apply 2 to 3 times, The interface agent coating covers the cement-based infiltrative crystallization material coating, and the edge of the interface agent coating exceeds the edge of the cement-based infiltrative crystallization material coating by 2 to 3 cm.

7. The repair construction method for small box beam wet joint cracking and whitening disease according to claim 1 or 6, characterized in that: in, In step S40, the interface agent is a modified acrylic acid solution. The modified acrylic acid solution is an emulsion-like substance prepared by emulsification reaction of acrylic acid and a modifier using an emulsion polymerization method.

8. The repair construction method for cracking and whitening defects of small box beam wet joints according to claim 1 is characterized by: in, In step S50, the method of applying the polymer repair mortar is: using a spatula, a trowel or a gloved hand to apply the mortar. The polymer repair mortar coating covers the interface agent coating and the edge of the polymer repair mortar coating exceeds the interface agent coating by 2 to 3 cm.

9. The repair construction method for small box beam wet joint cracking and whitening disease according to claim 1 or 8, characterized in that: in, In step S50, the polymer repair mortar is a new type of concrete repair mortar. The novel concrete repair mortar has both the adhesion of polymer materials and the durability of inorganic materials. The thickness of the polymer repair mortar coating is 4 to 6 mm.

10. The repair construction method for small box beam wet joint cracking and whitening damage according to claim 1 is characterized by: in, In step S60, the curing method is: 24 hours after construction, covering the polymer repair mortar coating with plastic sheet for wet curing for at least 7 days, and regularly sprinkling water for curing.