Concrete truss and preparation method thereof
By combining modified coal gangue with polyisoprene and ortho-toluenesulfonamide, the compressive strength and flexural strength of concrete materials are improved, and the problem of insufficient performance of coal gangue concrete materials in the existing technology is solved, and coal Application of gangue in concrete trusses.
Patent Information
- Application Number
- CN202411211878.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-22
AI Technical Summary
The existing concrete materials with coal gangue as aggregate have poor compressive strength and flexural strength, which limits the application of coal gangue in concrete trusses.
Modified coal gangue is used as a component of concrete materials, and concrete materials with improved compressive strength and flexural strength are prepared by combining coal gangue with substances such as polyisoprene and o-toluenesulfonamide. The weight ratio of isoprene is 9~14:1, and the use of trans polyisoprene and cis polyisoprene, as well as the addition of water reducing agents to improve material properties.
The compressive strength and flexural strength of concrete materials have been significantly improved, and the widespread application of coal gangue in concrete trusses has been promoted. The use of modified coal gangue has reduced water absorption and enhanced the compactness of the material and the interface adhesion.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of concrete materials, and in particular to a concrete truss and a preparation method thereof. Background Art
[0002] Concrete trusses are structural components made of concrete. They have the advantages of strong bearing capacity, good durability, flexible design and high cost-effectiveness. They are widely used in the construction of bridges, industrial buildings and public facilities.
[0003] Coal gangue is one of the industrial solid wastes. Its large-scale accumulation is likely to cause many ecological problems, such as land occupation, water pollution and soil pollution. At present, the utilization of coal gangue has attracted widespread attention. For large-scale utilization of coal gangue, using it as concrete aggregate is one of the most effective ways.
[0004] However, concrete materials with coal gangue as aggregate often show low compressive and flexural strength. Since the performance of concrete trusses is directly affected by the quality of the concrete materials used, improving the compressive and flexural strength of such concrete materials is crucial to promote the application of coal gangue in concrete trusses. Summary of the invention
[0005] The present invention provides a concrete truss and a preparation method thereof, which solves the problem that the concrete material containing coal gangue as aggregate used in the concrete truss in the related art has poor compressive strength and flexural strength.
[0006] The technical solution of the present invention is as follows: The present invention provides a concrete truss, which is cast by concrete materials, wherein the concrete materials include the following components in parts by weight: 20-30 parts of cement, 70-80 parts of quartz sand, 50-60 parts of modified coal gangue, 40-50 parts of granite powder, 1-2 parts of water reducing agent, and 15-25 parts of water; The modified coal gangue comprises coal gangue and polyisoprene.
[0007] As a further technical solution, the weight ratio of the coal gangue to polyisoprene is 9-14:1.
[0008] In the present invention, when the weight ratio of coal gangue to polyisoprene is 9-14:1, it helps to further improve the compressive strength and flexural strength of the concrete material, and further promotes the application of coal gangue in concrete trusses.
[0009] As a further technical solution, the preparation method of the modified coal gangue comprises the following steps: melting polyisoprene, adding coal gangue, dispersing evenly, and cooling to obtain the modified coal gangue.
[0010] As a further technical solution, during the melting, the temperature is 190-200°C.
[0011] As a further technical solution, the polyisoprene includes cis-polyisoprene and trans-polyisoprene.
[0012] In the present invention, when the polyisoprene includes cis-polyisoprene and trans-polyisoprene, the surface properties of coal gangue can be further enhanced by using two polyisoprenes with different structures in combination, thereby further improving the compressive strength and flexural strength of concrete materials, and further promoting the application of coal gangue in concrete trusses.
[0013] As a further technical solution, the weight of the trans-polyisoprene is greater than the weight of the cis-polyisoprene.
[0014] In the present invention, when the weight of trans-polyisoprene is greater than that of cis-polyisoprene, it helps to further improve the compressive strength and flexural strength of the concrete material, and further promotes the application of coal gangue in concrete trusses.
[0015] As a further technical solution, the modified coal gangue components also include o-toluenesulfonamide.
[0016] In the present invention, although the compressive strength and flexural strength of concrete materials can be improved by modifying coal gangue with polyisoprene, the inventors found that when the modified coal gangue also includes o-toluenesulfonamide, the compressive strength and flexural strength of concrete materials can be further improved. It is speculated that this is because o-toluenesulfonamide can improve the bonding ability between polyisoprene and coal gangue, further promoting the application of coal gangue in concrete trusses.
[0017] As a further technical solution, the weight ratio of the sum of the weights of the coal gangue and polyisoprene to the weight of the o-toluenesulfonamide is 5-11:1.
[0018] In the present invention, when the weight ratio of the sum of the weights of coal gangue and polyisoprene to the weight of o-toluenesulfonamide is 5-11:1, it helps to further improve the compressive strength and flexural strength of the concrete material, and further promotes the application of coal gangue in concrete trusses.
[0019] As a further technical solution, the preparation method of the modified coal gangue comprises the following steps: S1. Dissolve o-toluenesulfonamide in ethanol, add coal gangue, disperse evenly, and dry to obtain a precursor; S2, melting polyisoprene, adding the precursor, dispersing evenly, cooling, and obtaining the modified coal gangue.
[0020] As a further technical solution, in step S2, the temperature during melting is 190-200°C.
[0021] As a further technical solution, the water reducer is a polycarboxylic acid water reducer or a naphthalene-based water reducer.
[0022] In the present invention, the addition of a water reducer can improve the workability of the concrete material, thereby facilitating the improvement of the compressive strength and flexural strength of the concrete material. The polycarboxylate water reducer can be selected from Melflux-4930F, TD-JSS and TXHG-008, etc.; the naphthalene water reducer can be selected from TD-NX1 or FDN-C, etc., preferably a polycarboxylate water reducer, more preferably Melflux-4930F.
[0023] As a further technical solution, the particle size of the quartz sand is 6-8 mm; The particle size of the coal gangue is 3-4 mm; The particle size of the granite powder is 0.25-0.5 mm.
[0024] In the present invention, by rationally designing the aggregate gradation, voids can be reduced, the density of the concrete material can be improved, and thus the compressive strength and flexural strength of the concrete material can be improved.
[0025] The present invention also proposes a method for preparing a concrete truss, comprising the following steps: mixing the components evenly to obtain a concrete material, and casting and curing the concrete material to obtain a concrete truss.
[0026] As a further technical solution, the curing is carried out by natural curing for 14 to 21 days.
[0027] The working principle and beneficial effects of the present invention are: In the present invention, the concrete material containing coal gangue as aggregate used in the concrete truss has good compressive strength and flexural strength, which promotes the application of coal gangue in concrete trusses. Among them, the coal gangue is modified by polyisoprene, the water absorption of the coal gangue is reduced, and the problem of loosening of the coal gangue after absorbing water and causing weak interface bonding between the coal gangue and cement mortar is effectively avoided, so that the concrete material can better disperse stress when subjected to external force, reduce the possibility of stress concentration, and thus improve the compressive strength and flexural strength of the concrete material. DETAILED DESCRIPTION
[0028] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] In the following examples and comparative examples, unless otherwise specified, cement is ordinary Portland cement with a grade of P·O42.5R; the particle size of quartz sand is 7 mm, and the content of silicon dioxide is 96 wt %; the particle size of coal gangue is 3.5 mm, the content of silicon dioxide is 63 wt %, and the content of aluminum oxide is 18 wt %; the particle size of granite powder is 0.5 mm, and the content of silicon dioxide is 78 wt %; the model of cis-polyisoprene is IR2200L; the model of trans-polyisoprene is TPI-30; the water reducer is Melflux-4930F polycarboxylate water reducer; and the model of cis-polybutadiene is RB830.
[0030] Example 1 A method for preparing a concrete truss comprises the following steps: by weight, 20 parts of cement, 70 parts of quartz sand, 50 parts of modified coal gangue, 40 parts of granite powder, 1 part of water reducer and 15 parts of water are uniformly mixed to obtain a concrete material, and after the concrete material is poured, it is naturally cured for 21 days to obtain a concrete truss; The preparation method of modified coal gangue comprises the following steps: melting 1 part of cis-polyisoprene at 200° C., adding 49 parts of coal gangue, dispersing evenly, cooling, and obtaining modified coal gangue.
[0031] Example 2 A method for preparing a concrete truss comprises the following steps: mixing 30 parts of cement, 80 parts of quartz sand, 60 parts of modified coal gangue, 50 parts of granite powder, 2 parts of water reducing agent and 25 parts of water uniformly by weight to obtain a concrete material; after pouring the concrete material, naturally curing for 21 days to obtain a concrete truss; The preparation method of modified coal gangue comprises the following steps: melting 2 parts of cis-polyisoprene at 200° C., adding 58 parts of coal gangue, dispersing evenly, cooling, and obtaining modified coal gangue.
[0032] Example 3 The only difference between this embodiment and embodiment 2 is that in this embodiment, when preparing the modified coal gangue, the weight parts of cis-polyisoprene are 9 parts and the weight parts of coal gangue are 51 parts.
[0033] Example 4 The only difference between this embodiment and embodiment 2 is that in this embodiment, when preparing the modified coal gangue, the weight parts of cis-polyisoprene are 4 parts and the weight parts of coal gangue are 56 parts.
[0034] Example 5 The only difference between this embodiment and embodiment 2 is that in this embodiment, when preparing the modified coal gangue, the weight parts of cis-polyisoprene are 6 parts and the weight parts of coal gangue are 54 parts.
[0035] Example 6 The only difference between this example and Example 5 is that, in this example, cis-polyisoprene is replaced with an equal amount of trans-polyisoprene.
[0036] Example 7 The only difference between this example and example 5 is that in this example, 6 parts of cis-polyisoprene are replaced by 4 parts of cis-polyisoprene and 2 parts of trans-polyisoprene.
[0037] Example 8 The only difference between this example and Example 5 is that in this example, 6 parts of cis-polyisoprene are replaced by 3 parts of cis-polyisoprene and 3 parts of trans-polyisoprene.
[0038] Example 9 The only difference between this example and example 5 is that in this example, 6 parts of cis-polyisoprene are replaced by 2 parts of cis-polyisoprene and 4 parts of trans-polyisoprene.
[0039] Example 10 The difference between this embodiment and embodiment 5 is that in this embodiment, the preparation method of modified coal gangue includes the following steps: S1, dissolving 15 parts of o-toluenesulfonamide in 100 parts of ethanol, adding 40.5 parts of coal gangue, dispersing evenly, and drying to obtain a precursor; S2. Melt 4.5 parts of cis-polyisoprene at 200° C., add the above precursor, disperse evenly, and cool to obtain modified coal gangue.
[0040] Embodiment 11 The only difference between this embodiment and embodiment 10 is that in this embodiment, the weight portion of o-toluenesulfonamide is 2.5 parts, the weight portion of coal gangue is 51.75 parts, and the weight portion of cis-polyisoprene is 5.75 parts.
[0041] Example 12 The only difference between this embodiment and embodiment 10 is that in this embodiment, the weight parts of o-toluenesulfonamide are 10 parts, the weight parts of coal gangue are 45 parts, and the weight parts of cis-polyisoprene are 5 parts.
[0042] Example 13 The only difference between this embodiment and embodiment 10 is that, in this embodiment, the weight portion of o-toluenesulfonamide is 5 parts, the weight portion of coal gangue is 49.5 parts, and the weight portion of cis-polyisoprene is 5.5 parts.
[0043] Comparative Example 1 The only difference between this comparative example and Example 1 is that in this comparative example, the modified coal gangue is replaced by an equal amount of coal gangue.
[0044] Comparative Example 2 The only difference between this comparative example and Example 1 is that in this comparative example, the preparation method of modified coal gangue includes the following steps: melting 1 part of cis-polybutadiene at 200° C., adding 49 parts of coal gangue, dispersing evenly, and cooling to obtain modified coal gangue.
[0045] The concrete materials in Examples 1 to 13 and Comparative Examples 1 to 2 were cured according to the curing method of the specimens in GB / T 50081-2019 "Standard for Test Methods for Physical and Mechanical Properties of Concrete", and the curing age was 21 days. The following performance tests were performed on the cured concrete, and the arithmetic mean of the test results of 3 specimens in each group was taken as the final result, retaining 1 decimal place: ① Compressive strength: The compressive strength is measured according to GB / T 50081-2019 "Standard for Test Methods for Physical and Mechanical Properties of Concrete", where the loading speed is 0.8MPa / s; ② Flexural strength: The flexural strength is measured according to GB / T 50081-2019 "Standard for Test Methods for Physical and Mechanical Properties of Concrete", where the loading speed is 0.08 MPa / s.
[0046] The test results are shown in Table 1 below.
[0047]
[0048] The comparison between Example 1 and Comparative Examples 1-2 shows that the compression strength and flexural strength of concrete materials can be significantly improved by modifying coal gangue with polyisoprene. The comparison between Examples 2-3 and Examples 4-5 shows that when the weight ratio of coal gangue to polyisoprene is 9-14:1, it helps to further improve the compression strength and flexural strength of concrete materials. The comparison between Examples 5-6 and Examples 7-9 shows that when polyisoprene includes cis-polyisoprene and trans-polyisoprene, the compression strength and flexural strength of concrete materials can be further improved. The comparison between Example 9 and Examples 7-8 shows that when the weight of trans-polyisoprene is greater than the weight of cis-polyisoprene, it helps to further improve the compression strength and flexural strength of concrete materials. The comparison between Example 5 and Examples 10-13 shows that when the components of the modified coal gangue also include o-toluenesulfonamide, the compression strength and flexural strength of concrete materials can be further improved. Comparison between Examples 10-11 and Examples 12-13 shows that when the weight ratio of the sum of the weights of coal gangue and polyisoprene to the weight of o-toluenesulfonamide is 5-11:1, it helps to further improve the compressive strength and flexural strength of the concrete material.
[0049] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A concrete truss is made of concrete material. It is characterized in that The concrete material includes the following components in parts by weight: 20-30 parts of cement, 70-80 parts of quartz sand, 50-60 parts of modified coal gangue, 40-50 parts of granite powder, 1-2 parts of water reducing agent, and 15-25 parts of water; The modified coal gangue comprises coal gangue and polyisoprene.
2. A concrete truss according to claim 1, It is characterized in that The weight ratio of the coal gangue to polyisoprene is 9-14:
1.
3. A concrete truss according to claim 1, It is characterized in that The preparation method of the modified coal gangue comprises the following steps: melting polyisoprene, adding coal gangue, dispersing evenly, and cooling to obtain the modified coal gangue.
4. A concrete truss according to claim 1, It is characterized in that The polyisoprene includes cis-polyisoprene and trans-polyisoprene.
5. A concrete truss according to claim 1, It is characterized in that The modified coal gangue also includes o-toluenesulfonamide as a component.
6. A concrete truss according to claim 5, It is characterized in that The weight ratio of the sum of the weights of the coal gangue and polyisoprene to the weight of the o-toluenesulfonamide is 5-11:
1.
7. A concrete truss according to claim 5, It is characterized in that The preparation method of the modified coal gangue comprises the following steps: S1. Dissolve o-toluenesulfonamide in ethanol, add coal gangue, disperse evenly, and dry to obtain a precursor; S2, melting polyisoprene, adding the precursor, dispersing evenly, cooling, and obtaining the modified coal gangue.
8. A concrete truss according to any one of claims 1 to 7, It is characterized in that The water reducer is a polycarboxylate water reducer or a naphthalene water reducer.
9. A method for preparing a concrete truss according to any one of claims 1 to 8, It is characterized in that The following steps are involved: The components are mixed evenly to obtain a concrete material, and the concrete material is poured and cured to obtain a concrete truss.
10. A method for preparing a concrete truss according to claim 9, It is characterized in that During the curing, natural curing is adopted, and the time is 14 to 21 days.
Citation Information
Cited By
Asphalt modified coal gangue cement concrete and preparation method thereof
CN120328936A
Asphalt modified coal gangue cement concrete and preparation method thereof